5 中英文对照 土木工程 外文翻译 英文文献-混凝土应力实验

合集下载

完整版土木工程专业英语课文原文及对照翻译

完整版土木工程专业英语课文原文及对照翻译

Civil EngineeringCivil engineering, the oldest of the engineering specialties, is the planning, design, construction, and management of the built environment. This environment includes all structures built according to scientific principles, from irrigation and drainage systems to rocket-launching facilities.土木工程学作为最老的工程技术学科,是指规划,设计,施工及对建筑环境的管理。

此处的环境包括建筑吻合科学规范的所有结构,从灌溉和排水系统到火箭发射设施。

Civil engineers build roads, bridges, tunnels, dams, harbors, power plants, water and sewage systems, hospitals, schools, mass transit, and other public facilities essential to modern society and large population concentrations. They also build privately owned facilities such as airports, railroads, pipelines, skyscrapers, and other large structures designed for industrial, commercial, or residential use. In addition, civil engineers plan, design, and build complete cities and towns, and more recently have been planning and designing space platforms to house self-contained communities.土木工程师建筑道路,桥梁,管道,大坝,海港,发电厂,给排水系统,医院,学校,公共交通和其他现代社会和大量人口集中地区的基础公共设施。

土木工程英语文献原文及中文翻译

土木工程英语文献原文及中文翻译

Civil engineering introduction papers[英语原文]Abstract: the civil engineering is a huge discipline, but the main one is building, building whether in China or abroad, has a long history, long-term development process. The world is changing every day, but the building also along with the progress of science and development. Mechanics findings, material of update, ever more scientific technology into the building. But before a room with a tile to cover the top of the house, now for comfort, different ideas, different scientific, promoted the development of civil engineering, making it more perfect.[key words] : civil engineering; Architecture; Mechanics, Materials.Civil engineering is build various projects collectively. It was meant to be and "military project" corresponding. In English the history of Civil Engineering, mechanical Engineering, electrical Engineering, chemical Engineering belong to to Engineering, because they all have MinYongXing. Later, as the project development of science and technology, mechanical, electrical, chemical has gradually formed independent scientific, to Engineering became Civil Engineering of specialized nouns. So far, in English, to Engineering include water conservancy project, port Engineering, While in our country, water conservancy projects and port projects also become very close and civil engineering relatively independent branch. Civil engineering construction of object, both refers to that built on the ground, underground water engineering facilities, also refers to applied materials equipment and conduct of the investigation, design and construction, maintenance, repair and other professional technology.Civil engineering is a kind of with people's food, clothing, shelter and transportation has close relation of the project. Among them with "live" relationship is directly. Because, to solve the "live" problem must build various types of buildings. To solve the "line, food and clothes" problem both direct side, but also a indirect side. "Line", must build railways, roads, Bridges, "Feed", must be well drilling water, water conservancy, farm irrigation, drainage water supply for the city, that is direct relation. Indirectly relationship is no matter what you do, manufacturing cars, ships, or spinning and weaving, clothing, or even production steel, launch satellites, conducting scientific research activities are inseparable from build various buildings, structures and build all kinds of project facilities.Civil engineering with the progress of human society and development, yet has evolved into large-scale comprehensive discipline, it has out many branch, such as: architectural engineering, the railway engineering, road engineering, bridge engineering, special engineering structure, waterand wastewater engineering, port engineering, hydraulic engineering, environment engineering disciplines. [1]Civil engineering as an important basic disciplines, and has its important attributes of: integrated, sociality, practicality, unity. Civil engineering for the development of national economy and the improvement of people's life provides an important material and technical basis, for many industrial invigoration played a role in promoting, engineering construction is the formation of a fixed asset basic production process, therefore, construction and real estate become in many countries and regions, economic powerhouses.Construction project is housing planning, survey, design, construction of the floorboard. Purpose is for human life and production provide places.Houses will be like a man, it's like a man's life planning environment is responsible by the planners, Its layout and artistic processing, corresponding to the body shape looks and temperament, is responsible by the architect, Its structure is like a person's bones and life expectancy, the structural engineer is responsible, Its water, heating ventilation and electrical facilities such as the human organ and the nerve, is by the equipment engineer is responsible for. Also like nature intact shaped like people, in the city I district planning based on build houses, and is the construction unit, reconnaissance unit, design unit of various design engineers and construction units comprehensive coordination and cooperation process.After all, but is structural stress body reaction force and the internal stress and how external force balance. Building to tackle, also must solve the problem is mechanical problems. We have to solve the problem of discipline called architectural mechanics. Architectural mechanics have can be divided into: statics, material mechanics and structural mechanics three mechanical system. Architectural mechanics is discussion and research building structure and component in load and other factors affecting the working condition of, also is the building of intensity, stiffness and stability. In load, bear load and load of structure and component can cause the surrounding objects in their function, and the object itself by the load effect and deformation, and there is the possibility of damage, but the structure itself has certain resistance to deformation and destruction of competence, and the bearing capacity of the structure size is and component of materials, cross section, and the structural properties of geometry size, working conditions and structure circumstance relevant. While these relationships can be improved by mechanics formula solved through calculation.Building materials in building and has a pivotal role. Building material is with human society productivity and science and technologyimproves gradually developed. In ancient times, the human lives, the line USES is the rocks andTrees. The 4th century BC, 12 ~ has created a tile and brick, humans are only useful synthetic materials made of housing. The 17th century had cast iron and ShouTie later, until the eighteenth century had Portland cement, just make later reinforced concrete engineering get vigorous development. Now all sorts of high-strength structural materials, new decoration materials and waterproof material development, criterion and 20th century since mid organic polymer materials in civil engineering are closely related to the widely application. In all materials, the most main and most popular is steel, concrete, lumber, masonry. In recent years, by using two kinds of material advantage, will make them together, the combination of structure was developed. Now, architecture, engineering quality fit and unfit quality usually adopted materials quality, performance and using reasonable or not have direct connection, in meet the same technical indicators and quality requirements, under the precondition of choice of different material is different, use method of engineering cost has direct impact.In construction process, building construction is and architectural mechanics, building materials also important links. Construction is to the mind of the designer, intention and idea into realistic process, from the ancient hole JuChao place to now skyscrapers, from rural to urban country road elevated road all need through "construction" means. A construction project, including many jobs such as dredging engineering, deep foundation pit bracing engineering, foundation engineering, reinforced concrete structure engineering, structural lifting project, waterproofing, decorate projects, each type of project has its own rules, all need according to different construction object and construction environment conditions using relevant construction technology, in work-site.whenever while, need and the relevant hydropower and other equipment composition of a whole, each project between reasonable organizing and coordination, better play investment benefit. Civil engineering construction in the benefit, while also issued by the state in strict accordance with the relevant construction technology standard, thus further enhance China's construction level to ensure construction quality, reduce the cost for the project.Any building built on the surface of the earth all strata, building weight eventually to stratum, have to bear. Formation Support building the rocks were referred to as foundation, and the buildings on the ground and under the upper structure of self-respect and liable to load transfer to the foundation of components or component called foundation. Foundation, and the foundation and the superstructure is a building of three inseparable part. According to the function is different, but in load, under the action of them are related to each other, is theinteraction of the whole. Foundation can be divided into natural foundation and artificial foundation, basic according to the buried depth is divided into deep foundation and shallow foundation. , foundation and foundation is the guarantee of the quality of the buildings and normal use close button, where buildings foundation in building under loads of both must maintain overall stability and if the settlement of foundation produce in building scope permitted inside, and foundation itself should have sufficient strength, stiffness and durability, also consider repair methods and the necessary foundation soil retaining retaining water and relevant measures. [3]As people living standard rise ceaselessly, the people to their place of building space has become not only from the number, and put forward higher requirement from quality are put car higher demands that the environment is beautiful, have certain comfort. This needs to decorate a building to be necessary. If architecture major engineering constitutes the skeleton of the building, then after adornment building has become the flesh-and-blood organism, final with rich, perfect appearance in people's in front, the best architecture should fully embody all sorts of adornment material related properties, with existing construction technology, the most effective gimmick, to achieve conception must express effect. Building outfit fix to consider the architectural space use requirement, protect the subject institutions from damage, give a person with beautifulenjoying, satisfy the requirements of fire evacuation, decorative materials and scheme of rationality, construction technology and economic feasibility, etc. Housing construction development and at the same time, like housing construction as affecting people life of roads, Bridges, tunnels has made great progress.In general civil engineering is one of the oldest subjects, it has made great achievements, the future of the civil engineering will occupy in people's life more important position. The environment worsening population increase, people to fight for survival, to strive for a more comfortable living environment, and will pay more attention to civil engineering. In the near future, some major projects extimated to build, insert roller skyscrapers, across the oceanBridges, more convenient traffic would not dream. The development of science and technology, and the earth is deteriorating environment will be prompted civil engineering to aerospace and Marine development, provide mankind broader space of living. In recent years, engineering materials mainly is reinforced concrete, lumber and brick materials, in the future, the traditional materials will be improved, more suitable for some new building materials market, especially the chemistry materials will promote the construction of towards a higher point. Meanwhile, design method of precision, design work of automation, information and intelligent technology of introducing, will be people have a morecomfortable living environment. The word, and the development of the theory and new materials, the emergence of the application of computer, high-tech introduction to wait to will make civil engineering have a new leap.This is a door needs calm and a great deal of patience and attentive professional. Because hundreds of thousands, even hundreds of thousands of lines to building each place structure clearly reflected. Without a gentle state of mind, do what thing just floating on the surface, to any a building structure, to be engaged in business and could not have had a clear, accurate and profound understanding of, the nature is no good. In this business, probably not burn the midnight oil of courage, not to reach the goal of spirit not to give up, will only be companies eliminated.This is a responsible and caring industry. Should have a single responsible heart - I one's life in my hand, thousands of life in my hand. Since the civil, should choose dependably shoulder the responsibility.Finally, this is a constant pursuit of perfect industry. Pyramid, spectacular now: The Great Wall, the majestic... But if no generations of the pursuit of today, we may also use the sort of the oldest way to build this same architecture. Design a building structure is numerous, but this is all experienced centuries of clarification, through continuous accumulation, keep improving, innovation obtained. And such pursuit, not confined in the past. Just think, if the design of a building can be like calculation one plus one equals two as simple and easy to grasp, that was not for what? Therefore, a civil engineer is in constant of in formation. One of the most simple structure, the least cost, the biggest function. Choose civil, choosing a steadfast diligence, innovation, pursuit of perfect path.Reference:[1] LuoFuWu editor. Civil engineering (professional). Introduction to wuhan. Wuhan university of technology press. 2007[2] WangFuChuan, palace rice expensive editor. Construction engineering materials. Beijing. Science and technology literature press. 2002[3] jiang see whales, zhiming editor. Civil engineering introduction of higher education press. Beijing.. 1992土木工程概论 [译文]摘要:土木工程是个庞大的学科,但最主要的是建筑,建筑无论是在中国还是在国外,都有着悠久的历史,长期的发展历程。

土木工程英文文献及翻译-英语论文.doc

土木工程英文文献及翻译-英语论文.doc

土木工程英文文献及翻译-英语论文土木工程英文文献及翻译in Nanjing, ChinaZhou Jin, Wu Yezheng *, Yan GangDepartment of Refrigeration and Cryogenic Engineering, School of Energy and Power Engineering, Xi’an Jiao Tong University,Xi’an , PR ChinaReceived 4 April 2005; accepted 2 October 2005Available online 1 December 2005AbstractThe bin method, as one of the well known and simple steady state methods used to predict heating and cooling energyconsumption of buildings, requires reliable and detailed bin data. Since the long term hourly temperature records are notavailable in China, there is a lack of bin weather data for study and use. In order to keep the bin method practical in China,a stochastic model using only the daily maximum and minimum temperatures to generate bin weather data was establishedand tested by applying one year of measured hourly ambient temperature data in Nanjing, China. By comparison with themeasured values, the bin weather data generated by the model shows adequate accuracy. This stochastic model can be usedto estimate the bin weather data in areas, especially in China, where the long term hourly temperature records are missingor not available.Ó 2005 Elsevier Ltd. All rights reserved.Keywords: Energy analysis; Stochastic method; Bin data; China1. IntroductionIn the sense of minimizing the life cycle cost of a building, energy analysis plays an important role in devel-oping an optimum and cost effective design of a heating or an air conditioning system for a building. Severalmodels are available for estimating energy use in buildings. These models range from simple steady state mod-els to comprehensive dynamic simulation procedures.Today, several computer programs, in which the influence of many parameters that are mainly functionsof time are taken into consideration, are available for simulating both buildings and systems and performinghour by hour energy calculations using hourly weather data. DOE-2, BLAST and TRNSYS are such* Corresponding author. Tel.: +86 29 8266 8738; fax: +86 29 8266 8725.E-mail address: yzwu@ (W. Yezheng).0196-8904/$ - see front matter Ó 2005 Elsevier Ltd. All rights reserved.doi:10.1016/NomenclatureZ. Jin et al. / Energy Conversion and Management 47 (2006) 1843–1850number of daysfrequency of normalized hourly ambient temperatureMAPE mean absolute percentage error (%)number of subintervals into which the interval [0, 1] was equally dividednumber of normalized temperatures that fall in subintervalprobability densityhourly ambient temperature (°C)normalized hourly ambient temperature (dimensionless)weighting factorSubscriptscalculated valuemeasured valuemax daily maximummin daily minimumprograms that have gained widespread acceptance as reliable estimation tools. Unfortunately, along withthe increased sophistication of these models, they have also become very complex and tedious touse [1].The steady state methods, which are also called single measure methods, require less data and provideadequate results for simple systems and applications. These methods are appropriate if the utilization ofthe building can be considered constant. Among these methods are the degree day and bin data methods.The degree-day methods are the best known and the simplest methods among the steady state models.Traditionally, the degree-day method is based on the assumption that on a long term average, the solarand internal gains will offset the heat loss when the mean daily outdoor temperature is 18.3 °C and thatthe energy consumption will be proportional to the difference between 18.3 °C and the mean daily tempera-ture. The degree-day method can estimate energy consumption very accurately if the building use and theefficiency of the HVAC equipment are sufficiently constant. However, for many applications, at least oneof the above parameters varies with time. For instance, the efficiency of a heat pump system and HVAC equip-ment may be affected directly or indirectly by outdoor temperature. In such cases, the bin method can yieldgood results for the annual energy consumption if different temperature intervals and time periods areevaluated separately. In the bin method, the energy consumption is calculated for several values of the outdoortemperature and multiplied by the number of hours in the temperature interval (bin) centered around thattemperature. Bin data is defined as the number of hours that the ambient temperature was in each of a setof equally sized intervals of ambient temperature.In the United States, the necessary bin weather data are available in the literature [2,3]. Some researchers[4–8] have developed bin weather data for other regions of the world. However, there is a lack of informationin the ASHRAE handbooks concerning the bin weather data required to perform energy calculations in build-ings in China. The practice of analysis of weather data for the design of HVAC systems and energy consump-tion predictions in China is quite new. For a long time, only the daily value of meteorological elements, such asdaily maximum, minimum and average temperature, was recorded and available in most meteorologicalobservations in China, but what was needed to obtain the bin weather data, such as temperature bin data,were the long term hourly values of air temperature. The study of bin weather data is very limited in China.Only a few attempts [9,10] in which bin weather data for several cities was given have been found in China.Obviously, this cannot meet the need for actual use and research. So, there is an urgent need for developing binweather data in China. The objective of this paper, therefore, is to study the hourly measured air temperaturedistribution and then to establish a model to generate bin weather data for the long term daily temperaturedata.2. Data usedZ. Jin et al. / Energy Conversion and Management 47 (2006) 1843–1850In this paper, to study the hourly ambient temperature variation and to establish and evaluate the model, aone year long hourly ambient temperature record for Nanjing in 2002 was used in the study. These data aretaken from the Climatological Center of Lukou Airport in Nanjing, which is located in the southeast of China(latitude 32.0°N, longitude 118.8°E, altitude 9 m).In addition, in order to create the bin weather data for Nanjing, typical weather year data was needed.Based on the long term meteorological data from 1961 to 1989 obtained from the China MeteorologicalAdministration, the typical weather year data for most cities in China has been studied in our former research[11] by means of the TMY (Typical Meteorological Year) method. The typical weather year for Nanjing isshown in Table 1. As only daily values of the meteorological elements were recorded and available in China,the data contained in the typical weather year data was also only daily values. In this study, the daily maxi-mum and minimum ambient temperature in the typical weather year data for Nanjing was used.3. Stochastic model to generate bin dataTraditionally, the generation of bin weather data needs long term hourly ambient temperature records.However, in the generation, the time information, namely the exact time that such a temperature occurredin a day, was omitted, and only the numerical value of the temperature was used. So, the value of each hourlyambient temperature can be treated as the independent random variable, and its distribution within the dailytemperature range can be analyzed by means of probability theory.3.1. Probability distribution of normalized hourly ambient temperatureSince the daily maximum and minimum temperatures and temperature range varied day by day, the con-cept of normalized hourly ambient temperature should be introduced to transform the hourly temperatures ineach day into a uniform scale. The new variable, normalized hourly ambient temperature is defined by^ ¼ttmintmaxtminwhere ^ may be termed the normalized hourly ambient temperature, tmaxand tminare the daily maximum andminimum temperatures, respectively, t is the hourly ambient temperature. Obviously, the normalized hourly ambient temperature ^ is a random variable that lies in the interval [0, 1].To analyze its distribution, the interval [0, 1] can be divided equally into several subintervals, and by means ofthe histogram method [12]iin each subinterval can be calculated by1137土木工程英文文献及翻译Based on the one year long hourly ambient temperature data in Nanjing, China, the probability density piwas calculated for the whole day and the 08:00–20:00 period, where the interval [0, 1] was equally divided into50 subintervals, namely n equals 50. The results are shown in Fig. 1.According to the discrete probability density data in Fig. 1, the probability density function of ^ can beobtained by a fitting method. In this study, the quadratic polynomialswere used to fit the probability density data, where a, b and c are coefficients. According to the property of theprobability density function, the following equation should be satisfiedAs shown in Fig. 1, the probability density curve obtained according to the probability density data pointsis also shown. The probability densit y functions that are fitted are described byp ¼ 2:7893^23:1228^ þ 1:6316 for the whole day periodp ¼ 2:2173^20:1827^ þ 0:3522 for the 08 : 00–20 : 00 period3.2. The generation of hourly ambient temperatureAs stated in the beginning of this paper, the objective of this study is to generate the hourly ambient tem-perature needed for bin weather data generation in the case that only the daily maximum and minimum tem-peratures are known. To do this, we can use the obtained probability density function to generate thenormalized hourly ambient temperature and then transform it to hourly temperature. This belongs to theproblem of how to simulate a random variable with a prescribed probability density function and can be doneon a computer by the method described in the literature [13]. For a given probability density function f ð^Þ, ifits distribution function F ð^Þ can be obtained and if u is a random variable with uniform distribution on [0, 1],thenF, we need only setAs stated above, the probability density function of the normalized ambient temperature was fitted using aone year long hourly temperature data. Based on the probability density function obtained, the random nor-malized hourly temperature can be generated. When the daily maximum and minimum temperature areknown, the normalized hourly temperature can be transformed to an actual temperature by the followingequationWhen the hourly temperature for a particular period of the day has been generated using the above method,the bin data can also be obtained. Because the normalized temperature generated using the model in this studyis a random variable, the bin data obtained from each generation shows somedifference, but it has much sim-ilarity. To obtain a stable result of bin data, the generation of the bin data can be performed enough times,and the bin data can be obtained by averaging the result of each generation. In this paper, 50 generations wereaveraged to generate the bin weather data.Z. Jin et al. / Energy Conversion and Management 47 (2006) 1843–18503.4. Methods of model evaluationThe performance of the model was evaluated in terms of the following statistical error test:土木工程英文文献及翻译一种产生bin气象数据的随机方法——中国南京周晋摘要:bin方法是一种众所周知且简捷的稳态的计算方法,可以用来预计建筑的冷热能耗。

土木工程专业外文文献及翻译

土木工程专业外文文献及翻译

英文原文:Building construction concrete crack ofprevention and processingAbstractThe crack problem of concrete is a widespread existence but again difficult in solve of engineering actual problem, this text carried on a study analysis to a little bit familiar crack problem in the concrete engineering, and aim at concrete the circumstance put forward some prevention, processing measure.Keyword: Concrete crack prevention processingForewordConcrete's is 1 kind is anticipate by the freestone bone, cement, water and other mixture but formation of the in addition material of quality brittleness not and all material. Because the concrete construction transform with oneself, control etc. a series problem, harden model of in the concrete existence numerous tiny hole, spirit cave and tiny crack, is exactly because these beginning start blemish of existence just make the concrete present one some not and all the characteristic of quality. The tiny crack is a kind of harmless crack and accept concrete heavy, defend Shen and a little bit other use function not a creation to endanger. But after the concrete be subjected to lotus carry, difference in temperature etc. function, tiny crack would continuously of expand with connect, end formation we can see without the aid of instruments of macro view the crack be also the crack that the concrete often say in the engineering.Concrete building and Gou piece usually all take sewer to make of, because of crack of existence and development usually make inner part of reinforcing bar etc. material creation decay, lower reinforced concrete material of loading ability, durable and anti- Shen ability, influence building of external appearance, service life, severity will threat arrive people's life and property safety. A lot of all of crash of engineerings is because of the unsteady development of the crack with the resultthat. Modern age science research with a great deal of of the concrete engineering practice certificate, in the concrete engineering crack problem is ineluctable, also acceptable in certainly of the scope just need to adopt valid of measure will it endanger degree control at certain of scope inside. The reinforced concrete norm is also explicit provision: Some structure at place of dissimilarity under the condition allow existence certain the crack of width. But at under construction should as far as possible adopt a valid measure control crack creation, make the structure don't appear crack possibly or as far as possible decrease crack of amount and width, particularly want to as far as possible avoid harmful crack of emergence, insure engineering quality thus.Concrete crack creation of the reason be a lot of and have already transformed to cause of crack: Such as temperature variety, constringency, inflation, the asymmetry sink to sink etc. reason cause of crack; Have outside carry the crack that the function cause; Protected environment not appropriate the crack etc. caused with chemical effect. Want differentiation to treat in the actual engineering, workout a problem according to the actual circumstance.In the concrete engineering the familiar crack and the prevention1.Stem Suo crack and preventionStem the Suo crack much appear after the concrete protect be over of a period of time or concrete sprinkle to build to complete behind of around a week. In the cement syrup humidity of evaporate would creation stem Suo, and this kind of constringency is can't negative. Stem Suo crack of the creation be main is because of concrete inside outside humidity evaporate degree dissimilarity but cause to transform dissimilarity of result: The concrete is subjected to exterior condition of influence, surface humidity loss lead quick, transform bigger, inner part degree of humidity variety smaller transform smaller, bigger surface stem the Suo transform to be subjected to concrete inner part control, creation more big pull should dint but creation crack. The relative humidity is more low, cement syrup body stem Suo more big, stem the Suo crack be more easy creation. Stem the Suo crack is much surface parallel lines form or the net shallow thin crack, width many between 0.05-0.2 mm,the flat surface part much see in the big physical volume concrete and follow it more in thinner beam plank short to distribute. Stem Suo crack usually the anti- Shen of influence concrete, cause the durable of the rust eclipse influence concrete of reinforcing bar, under the function of the water pressure dint would creation the water power split crack influence concrete of loading dint etc..Concrete stem the Suo be main with water ash of the concrete ratio, the dosage of the composition, cement of cement, gather to anticipate of the dosage of the property and dosage, in addition etc. relevant.Main prevention measure: While being to choose to use the constringency quantity smaller cement, general low hot water mire and powder ash from stove cement in the adoption, lower the dosage of cement. Two is a concrete of stem the Suo be subjected to water ash ratio of influence more big, water ash ratio more big, stem Suo more big, so in the concrete match the ratio the design should as far as possible control good water ash ratio of choose to use, the Chan add in the meantime accommodation of reduce water. Three is strict control concrete mix blend with under construction of match ratio, use of concrete water quantity absolute can't big in match ratio design give settle of use water quantity. Four is the earlier period which strengthen concrete to protect, and appropriate extension protect of concrete time. Winter construction want to be appropriate extension concrete heat preservation to overlay time, and Tu2 Shua protect to protect. Five is a constitution the accommodation is in the concrete structure of the constringency sew.2.The Su constringency crack and preventionSu constringency is the concrete is before condense, surface because of lose water quicker but creation of constringency. The Su constringency crack is general at dry heat or strong wind the weather appear, crack's much presenting in the center breadth, both ends be in the center thin and the length be different, with each other not coherent appearance. Shorter crack general long 20-30 cm, the longer crack can reach to a 2-3 m, breadth 1-5 mm. It creation of main reason is: The concrete is eventually almost having no strength or strength before the Ning very small, perhapsconcrete just eventually Ning but strength very hour, be subjected to heat or compare strong wind dint of influence, the concrete surface lose water to lead quick, result in in the capillary creation bigger negative press but make a concrete physical volume sharply constringency, but at this time the strength of concrete again can't resist its constringency, therefore creation cracked. The influence concrete Su constringency open the main factor of crack to have water ash ratio, concrete of condense time, environment temperature, wind velocity, relative humidity...etc..Main prevention measure: One is choose to use stem the Suo value smaller higher Huo sour salt of the earlier period strength or common the Huo sour brine mire. Two is strict the control water ash ratio, the Chan add to efficiently reduce water to increment the collapse of concrete fall a degree and with easy, decrease cement and water of dosage. Three is to sprinkle before building concrete, water basic level and template even to soak through. Four is in time to overlay the perhaps damp grass mat of the plastics thin film, hemp slice etc., keep concrete eventually before the Ning surface is moist, perhaps spray to protect etc. to carry on protect in the concrete surface. Five is in the heat and strong wind the weather to want to establish to hide sun and block breeze facilities, protect in time.3.Sink to sink crack and preventionThe creation which sink to sink crack is because of the structure foundation soil quality not and evenly, loose soft or return to fill soil dishonest or soak in water but result in the asymmetry sink to decline with the result that; Perhaps because of template just degree shortage, the template propped up to once be apart from big or prop up bottom loose move etc. to cause, especially at winter, the template prop up at jelly soil up, jelly the soil turn jelly empress creation asymmetry to sink to decline and cause concrete structure creation crack. This kind crack many is deep enter or pierce through sex crack, it alignment have something to do with sinking to sink a circumstance, general follow with ground perpendicular or present 30 °s-45 °Cape direction development, bigger sink to sink crack, usually have certain of wrong, crack width usually with sink to decline quantity direct proportion relation. Crack width under the influence of temperature variety smaller. The foundation aftertransform stability sink to sink crack also basic tend in stability.Main prevention measure: One is rightness loose soft soil, return to fill soil foundation a construction at the upper part structure front should carry on necessity of Hang solid with reinforce. Two is the strength that assurance template is enough and just degree, and prop up firm, and make the foundation be subjected to dint even. Three is keep concrete from sprinkle infusing the foundation in the process is soak by water. Four is time that template tore down to can't be too early, and want to notice to dismantle a mold order of sequence. Five is at jelly soil top take to establish template to notice to adopt certain of prevention measure.4.Temperature crack and preventionTemperature crack much the occurrence is in big surface or difference in temperature variety of the physical volume concrete compare the earth area of the concrete structure. Concrete after sprinkling to build, in the hardening the process, cement water turn a creation a great deal of of water turn hot, .(be the cement dosage is in the 350-550 kg/m 3, each sign square the rice concrete will release a calories of 17500-27500 kJ and make concrete internal thus the temperature rise to reach to 70 ℃or so even higher)Because the physical volume of concrete be more big, a great deal of of water turn hot accumulate at the concrete inner part but not easy send forth, cause inner part the temperature hoick, but the concrete surface spread hot more quick, so formation inside outside of bigger difference in temperature, the bigger difference in temperature result in inner part and exterior hot the degree of the bulge cold Suo dissimilarity, make concrete surface creation certain of pull should dint.When pull should dint exceed the anti- of concrete pull strength extreme limit, concrete surface meeting creation crack, this kind of crack much occurrence after the concrete under construction period.In the concrete of under construction be difference in temperature variety more big, perhaps is a concrete to be subjected to assault of cold wave etc., will cause concrete surface the temperature sharply descend, but creation constringency, surface constringency of the concrete be subjected to inner part concrete of control, creation very big of pull should dint but creation crack, this kind of crack usually just in more shallow scope ofthe concrete surface creation.The alignment of the temperature crack usually none settle regulation, big area structure the crack often maneuver interleave;The size bigger structure of the beam plank length, the crack run parallel with short side more;Thorough with pierce through sex of temperature crack general and short side direction parallelism or close parallelism, crack along long side cent the segment appear, in the center more airtight.Crack width the size be different, be subjected to temperature variety influence more obvious, winter compare breadth, summer more narrow.The concrete temperature crack that the heat inflation cause is usually in the center the thick both ends be thin, but cold Suo crack of thick thin variety not too obvious.The emergence of the this kind crack will cause the rust eclipse of reinforcing bar, the carbonization of concrete, the anti- jelly which lower concrete melt, anti- tired and anti- Shen ability etc..Main prevention measure:One is as far as possible choose to use low hot or medium hot water mire, like mineral residue cement, powder ash from stove cement...etc..Two is a decrease cement dosage, cement dosage as far as possible the control is in the 450 kg/m 3 following.Three is to lower water ash ratio, water ash of the general concrete ratio control below 0.6.Four is improvement the bone anticipate class to go together with, the Chan add powder ash from stove or efficiently reduce water etc. to come to reduce cement dosage and lower water to turn hot.Five is an improvement concrete of mix blend to process a craft, lower sprinkle of concrete to build temperature.Six is the in addition that the Chan add a have of fixed amount to reduce water and increase Su, slow Ning etc. function in the concrete, improvement the concrete mix to match a thing of mobility, protect water, lower water to turn hot, postpone hot Feng of emergence time.Seven is the heat season sprinkle to build can the adoption take to establish to hide sun plank etc. assistance measure control concrete of Wen Sheng, lower to sprinkle temperature of build the concrete.Eight is the temperature of big physical volume concrete should the dint relate to structure size, concrete structure size more big, temperature should dint more big, so want reasonable arrangement construction work preface,layering, cent the piece sprinkle to build, for the convenience of in spread hot, let up control.Nine is at great inner part constitution of the physical volume concrete cool off piping, cold water perhaps cold air cool off, let up concrete of inside outside difference in temperature.Ten is the supervision which strengthen concrete temperature, adopt to cool off in time, protection measure.11 is to reserve temperature constringency to sew.12 is to let up to control, sprinkle proper before building concrete in the Ji rock and old concrete top build a 5 mm or so sand mat a layer or usage asphalt etc. material Tu2 Shua.13 is to strengthen concrete to protect, the concrete after sprinkle build use moist grass Lian in time, hemp slice's etc. overlay, and attention sprinkle water to protect, appropriate extension protect time, assurance the concrete surface be slow-moving cool off.At the cold season, concrete surface should constitution heat preservation measure, in order to prevent cold wave assault.14 is the allocation be a little amount in the concrete of reinforcing bar perhaps add fiber material concrete of temperature crack control at certain of scope inside.5.Crack and prevention that the chemical reaction causeAlkali bone's anticipating the crack that reaction crack and reinforcing bar rust eclipse cause is the most familiar in the reinforced concrete structure of because of chemical reaction but cause of crack.The concrete blend a future reunion creation some alkalescence ion, these ion with some activity the bone anticipate creation chemical reaction and absorb surroundings environment in of water but the physical volume enlarge, make concrete crisp loose, inflation open crack.In this kind of crack general emergence concrete structure usage period, once appear very difficult remediable, so should at under construction adopt valid the measure carry on prevention.Main of prevention measure:While being to choose to anticipate with the alkali activity small freestone bone.Two is the in addition which choose to use low lye mire with low alkali or have no alkali.Three is the Chan which choose to use accommodation with anticipate to repress an alkali bone to anticipate reaction.Because the concrete sprinkle to build, flap Dao bad perhaps is a reinforcingbar protection layer thinner, the harmful material get into concrete to make reinforcing bar creation rust eclipse, the reinforcing bar physical volume of the rust eclipse inflation, cause concrete bulge crack, the crack of this kind type much is a crack lengthways, follow the position of reinforcing bar ually of prevent measure from have:One is assurance reinforcing bar protection the thickness of the layer.Two is a concrete class to go together with to want good.Three is a concrete to sprinkle to note and flap Dao airtight solid.Four is a reinforcing bar surface layer Tu2 Shua antisepsis coating.Crack processingThe emergence of the crack not only would influence structure of whole with just degree, return will cause the rust eclipse of reinforcing bar, acceleration concrete of carbonization, lower durable and anti- of concrete tired, anti- Shen ability.Therefore according to the property of crack and concrete circumstance we want differentiation to treat, in time processing, with assurance building of safety usage.The repair measure of the concrete crack is main to have the following some method:Surface repair method, infuse syrup, the Qian sew method, the structure reinforce a method, concrete displacement method, electricity chemistry protection method and imitate to living from heal method.Surface repair the method be a kind of simple, familiar of repair method, it main be applicable to stability and to structure loading the ability don't have the surface crack of influence and deep enter crack of processing.The processing measure that is usually is a surface in crack daubery cement syrup, the wreath oxygen gum mire or at concrete surface Tu2 Shua paint, asphalt etc. antisepsis material, at protection of in the meantime for keeping concrete from continue under the influence of various function to open crack, usually can adoption the surface in crack glue to stick glass fiber cloth etc. measure.1, infuse syrup, the Qian sew methodInfuse a syrup method main the concrete crack been applicable to haveinfluence or have already defend Shen request to the structure whole of repair, it is make use of pressure equipments gum knot the material press into the crack of concrete, gum knot the material harden behind and concrete formation one be whole, thus reinforce of purpose.The in common use gum knot material has the cement the syrup, epoxy, A Ji C Xi sour ester and gather ammonia ester to equalize to learn material.The Qian sew a method is that the crack be a kind of most in common use method in, it usually is follow the crack dig slot, the Qian fill Su in the slot or rigid water material with attain closing crack of purpose.The in common use Su material has PVC gum mire, plastics ointment, the D Ji rubber etc.;In common use rigid water material is the polymer cement sand syrup.2, the structure reinforce a methodWhen the crack influence arrive concrete structure of function, will consideration adopt to reinforce a method to carry on processing to the concrete structure.The structure reinforce medium in common use main have the following a few method:The piece of enlargement concrete structure in every aspect accumulate, outside the Cape department of the Gou piece pack type steel, adoption prepare should the dint method reinforce, glue to stick steel plate to reinforce, increase to establish fulcrum to reinforce and jet the concrete compensation reinforce.3, concrete displacement methodConcrete displacement method is processing severity damage concrete of a kind of valid method, this method be first will damage of the concrete pick and get rid of, then again displacement go into new of concrete or other material.The in common use displacement material have:Common concrete or the cement sand syrup, polymer or change sex polymer concrete or sand syrup.4, the electricity chemistry protection methodThe electricity chemistry antisepsis is to make use of infliction electric field in lie the quality of electricity chemical effect, change concrete or reinforced concrete the environment appearance of the place, the bluntness turn reinforcing bar to attainthe purpose of antisepsis.Cathode protection method, chlorine salt's withdrawing a method, alkalescence to recover a method is a chemistry protection method in three kinds of in common use but valid method.The advantage of this kind of method is a protection method under the influence of environment factor smaller, apply reinforcing bar, concrete of long-term antisepsis, since can used for crack structure already can also used for new set up structure.5, imitate to living from legal moreImitate to living from heal the method be a kind of new crack treatment, its mimicry living creature organization secrete a certain material towards suffering wound part auto, but make the wound part heal of function, join some and special composition(such as contain to glue knot of the liquid Xin fiber or capsule) in the concrete of the tradition the composition, at concrete inner part formation the intelligence type imitate to living from heal nerve network system, be the concrete appear crack secrete a parts of liquid Xin fiber can make the crack re- heal.ConclusionThe crack is widespread in the concrete structure existence of a kind of phenomenon, it of emergence not only will lower the anti- Shen of building ability, influence building of usage function, and will cause the rust eclipse of reinforcing bar, the carbonization of concrete, lower the durable of material, influence building of loading ability, so want to carry on to the concrete crack earnest research, differentiation treat, adoption reasonable of the method carry on processing, and at under construction adopt various valid of prevention measure to prevention crack of emergence and development, assurance building and Gou piece safety, stability work.From《CANADIAN JOURNAL OF CIVIL ENGINEERING》中文原文:建筑施工混凝土裂缝的预防与处理混凝土的裂缝问题是一个普遍存在而又难于解决的工程实际问题,本文对混凝土工程中常见的一些裂缝问题进行了探讨分析,并针对具体情况提出了一些预防、处理措施。

土木工程 外文翻译 外文文献 英文文献

土木工程 外文翻译 外文文献 英文文献

一、外文原文Talling building and Steel construction Although there have been many advancements in building construction technology in general. Spectacular archievements have been made in the design and construction of ultrahigh-rise buildings.The early development of high-rise buildings began with structural steel framing.Reinforced concrete and stressed-skin tube systems have since been economically and competitively used in a number of structures for both residential and commercial purposes.The high-rise buildings ranging from 50 to 110 stories that are being built all over the United States are the result of innovations and development of new structual systems.Greater height entails increased column and beam sizes to make buildings more rigid so that under wind load they will not sway beyond an acceptable limit.Excessive lateral sway may cause serious recurring damage to partitions,ceilings.and other architectural details. In addition,excessive sway may cause discomfort to the occupants of the building because their perception of such motion.Structural systems of reinforced concrete,as well as steel,take full advantage of inherent potential stiffness of the total building and therefore require additional stiffening to limit the sway.In a steel structure,for example,the economy can be defined in terms of the total average quantity of steel per square foot of floor area of the building.Curve A in Fig .1 represents the average unit weight of a conventional frame with increasing numbers of stories. Curve B represents the average steel weight if the frame is protected from all lateral loads. The gap between the upper boundary and the lower boundary represents the premium for height for the traditional column-and-beam frame.Structural engineers have developed structural systems with a view to eliminating this premium.Systems in steel. Tall buildings in steel developed as a result ofseveral types of structural innovations. The innovations have been applied to the construction of both office and apartment buildings.Frame with rigid belt trusses. In order to tie the exterior columns of a frame structure to the interior vertical trusses,a system of rigid belt trusses at mid-height and at the top of the building may be used. A good example of this system is the First Wisconsin Bank Building(1974) in Milwaukee.Framed tube. The maximum efficiency of the total structure of a tall building, for both strength and stiffness,to resist wind load can be achieved only if all column element can be connected to each other in such a way that the entire building acts as a hollow tube or rigid box in projecting out of the ground. This particular structural system was probably used for the first time in the 43-story reinforced concrete DeWitt Chestnut Apartment Building in Chicago. The most significant use of this system is in the twin structural steel towers of the 110-story World Trade Center building in New York Column-diagonal truss tube. The exterior columns of a building can be spaced reasonably far apart and yet be made to work together as a tube by connecting them with diagonal members interesting at the centre line of the columns and beams. This simple yet extremely efficient system was used for the first time on the John Hancock Centre in Chicago, using as much steel as is normally needed for a traditional 40-story building.Bundled tube. With the continuing need for larger and taller buildings, the framed tube or the column-diagonal truss tube may be used in a bundled form to create larger tube envelopes while maintaining high efficiency. The 110-story Sears Roebuck Headquarters Building in Chicago has nine tube, bundled at the base of the building in three rows. Some of these individual tubes terminate at different heights of the building, demonstrating the unlimited architectural possibilities of this latest structural concept. The Sears tower, at a height of 1450 ft(442m), is the world’s tallest building.Stressed-skin tube system. The tube structural system was developed for improving the resistance to lateral forces (wind and earthquake) and thecontrol of drift (lateral building movement ) in high-rise building. The stressed-skin tube takes the tube system a step further. The development of the stressed-skin tube utilizes the façade of the building as a structural element which acts with the framed tube, thus providing an efficient way of resisting lateral loads in high-rise buildings, and resulting in cost-effective column-free interior space with a high ratio of net to gross floor area.Because of the contribution of the stressed-skin façade, the framed members of the tube require less mass, and are thus lighter and less expensive. All the typical columns and spandrel beams are standard rolled shapes,minimizing the use and cost of special built-up members. The depth requirement for the perimeter spandrel beams is also reduced, and the need for upset beams above floors, which would encroach on valuable space, is minimized. The structural system has been used on the 54-story One Mellon Bank Center in Pittburgh.Systems in concrete. While tall buildings constructed of steel had an early start, development of tall buildings of reinforced concrete progressed at a fast enough rate to provide a competitive chanllenge to structural steel systems for both office and apartment buildings.Framed tube. As discussed above, the first framed tube concept for tall buildings was used for the 43-story DeWitt Chestnut Apartment Building. In this building ,exterior columns were spaced at 5.5ft (1.68m) centers, and interior columns were used as needed to support the 8-in . -thick (20-m) flat-plate concrete slabs.Tube in tube. Another system in reinforced concrete for office buildings combines the traditional shear wall construction with an exterior framed tube. The system consists of an outer framed tube of very closely spaced columns and an interior rigid shear wall tube enclosing the central service area. The system known as the tube-in-tube system , made it possible to design the world’s present tallest (714ft or 218m)lightweight concrete bu ilding( the 52-story One Shell Plaza Building in Houston) for the unit price of a traditional shear wall structure of only 35 stories.Systems combining both concrete and steel have also been developed, an examle of which is the composite system developed by skidmore, Owings &Merril in which an exterior closely spaced framed tube in concrete envelops an interior steel framing, thereby combining the advantages of both reinforced concrete and structural steel systems. The 52-story One Shell Square Building in New Orleans is based on this system.Steel construction refers to a broad range of building construction in which steel plays the leading role. Most steel construction consists of large-scale buildings or engineering works, with the steel generally in the form of beams, girders, bars, plates, and other members shaped through the hot-rolled process. Despite the increased use of other materials, steel construction remained a major outlet for the steel industries of the U.S, U.K, U.S.S.R, Japan, West German, France, and other steel producers in the 1970s.二、原文翻译高层结构与钢结构近年来,尽管一般的建筑结构设计取得了很大的进步,但是取得显著成绩的还要属超高层建筑结构设计。

土木工程混凝土论文中英文资料外文翻译文献

土木工程混凝土论文中英文资料外文翻译文献

土木工程混凝土论文中英文资料外文翻译文献外文资料STUDIES ON IMPACT STRENGTH OF CONCRETESUBJECTED TO SUSTAINEDELEVATED TEMPERATUREConcrete has a remarkable fire resisting properties. Damage in concrete due to fire depends on a great extent on the intensity and duration of fire. Spalling cracking during heating are common concrete behaviour observed in the investigation of the fire affected structures. Plenty of literature is available on the studies of concrete based on time temperature cures. In power, oil sectorsand nuclear reactors concrete is exposed to high temperature for considerable period of time. These effects can be reckoned as exposure to sustained elevated temperature. The sustained elevated temperature may be varying from a few hours to a number of years depending upon practical condition of exposures. The knowledge on properties under such conditions is also of prime importance apart from the structures subjected to high intensity fire. Impact studies of structure subjected to sustained elevated temperature becomes more important as it involves sensitive structures which is more prone to attacks and accidents. In this paper impact studies on concrete subjected to sustained elevated temperature has been discussed. Experiments have been conducted on 180 specimens along with 180 companion cube specimens. The temperatures of 100°C, 200°C and 300°C for a duration of exposure of 2 hours 4 hours and 6 hours has been considered in the experiments. The results are logically analyzed and concluded.1. INTRODUCTIONThe remarkable property of concrete to resist the fire reduces the damage in a concrete structure whenever there is an accidental fire. In most of the cases the concrete remains intact with minor damages only. The reason being low thermal conductivity of concrete at higher temperatures and hence limiting the depth of penetration of firedamage. But when the concrete is subjected to high temperature for long duration the deterioration of concrete takes place. Hence it is essential to understand the strength and deformation characteristics of concrete subjected to temperature for long duration. In this paper an attempt has been made to study the variation in Impact Strength of concrete when subjected to a temperature range 100oC, 200oC and 300oC sustained for a period of 2 hrs, 4 hrs and 6 hrs.The review of the literature shows that a lot of research work [1 – 3] has taken place on the effect of elevated temperature on concrete. All these studies are based on time –temperature curves. Hence an attempt has been made to study the effect of sustained elevated temperature on impact strength of concrete and the results are compared with the compressive strength. The experimental programme has been planned for unstressed residual strength test based on the available facilities. Residual strength is the strength of heated and subsequently cooled concrete specimens expressed as percentage of the strength of unheated specimens.2. EXPERIMENTAL INVESTIGATION2.1. TEST SPECIMEN AND MATERIALSA total of 180 specimens were tested in the present study along with 180 companion cubes. An electric oven capable of reaching a maximum temperature of 300oC has been used for investigation. Fine and coarse aggregates conforming to IS383 has been used to prepare the specimen with mix proportions M1 = 1:2.1:3.95 w/c = 0.58, M2 = 1:1.15:3.56 w/c = 0.53, M3 = 1:0.8:2.4 w/c = 0.4.2.2 TEST VARIABLESThe effects of the following variables were studied.2.2.1 Size sSize of Impact Strength Test Specimen was 150 mm dial and 64 mm thickness and size of companion cube 150 x 150 x 150 mm.2.2.2 Maximum TemperatureIn addition to room temperature, the effect of three different temperatures (100oC, 200oC and 300oC) on the compressive strength was investigated.2.2.3 Exposure Time at Maximum TemperatureThree different exposure times were used to investigate the influence of heat on compressive strength; they are 2 hrs, 4 hrs and 6 hrs.2.2.4 Cooling MethodSpecimens were cooled in air to room temperature.3. TEST PROCEDUREAll the specimens were cast in steel moulds as per IS516 and each layer was compacted. Specimens were then kept in their moulds for 24 hours after which they were decoupled and placed into a curing tank until 28 days. After which the specimens were removed and were allowed to dry in room temperature. These specimens were kept in the oven and the required target temperature was set. Depending on the number of specimen kept inside the oven the time taken to reach the steady state was found to vary. After the steady state was reached the specimens were subjected to predetermined steady duration at the end of which the specimens are cooled to room temperature and tested.ACI drop weight impact strength test was adopted. This is the simplest method for evaluating impact resistance of concrete. The size of the specimen is 150 mm dial and 64 mm thickness. The disc specimens were prepared using steel moulds cured and heated and cooled as. This consists of a standard manually operated 4.54 kg hammer with 457 mm drop. A 64 mm hardened steel ball and a flat base plate with positioning bracket and lugs. The specimen is placed between the four guides pieces (lugs) located 4.8 mm away from the sample. A frame (positioning bracket) is then built in order to target the steel ball at the centre of concrete disc. The disc is coated at the bottom with a thin layer of petroleum jelly or heavy grease to reduce the friction between the specimen and base plate. The bottom part of the hammer unit was placed with its base upon the steel ball and the load was applied by dropping weight repeatedly. The loading was continued until the disc failed and opened up such that it touched three of the four positioning lugs. The number of blows that caused this condition is recorded as the failure strength. The companion cubes were tested for cube compression strength (fake).4. ANALYSIS AND RESULTS4.1 RESIDUAL COMPRESSIVE STRENGTH VS. TEMPERATUREFrom Table 1, at 100°C sustained elevated temperature it is seen that the residual strength of air cooled specimens of mixes M1, M2 and M3 has increased in strength 114% for M1 mix, 109% for M2 mix and 111% for M3 mix for 6 hours duration of exposure. When the sustained elevated temperature is to 200°C for air cooled specimens there is a decrease in strength up to 910% approximately for M1 mix for a duration of 6 hours, but in case of M2 mix it is 82% and for M3 mix it is 63% maximum for 6 hours duration of exposure. When the concrete mixes M1, M2 and M3 are exposed to 300°C sustained temperature there is a reduction in strength up to 78% for M1 mix for 6 hour duration of exposure.4.2 RESIDUAL COMPRESSIVE STRENGTH VS DURATION OF EXPOSUREFrom Table 1, result shows that heating up to 100°C for 2 hours and 4 hours, the residual strength of mix M1 has decreased where as the residual strength of mix M2 and M3 has increased. The residual strength is further increased for 6 hours duration of exposure in all the three mixes M1, M2 and M3 even beyond the strength at room temperature. When the specimens of mixes M1, M2 and M3 are exposed to 200°C for 2,4 and 6 hours of duration, it is observed that the residual strength has decreased below the room temperature and has reached 92% for M1 mix, 82 and 73% for M2 and M3 mix respectively. Concrete cubes of mixes M1, M2 and M3 when subjected to 300°C temperature for 2,4 and 6 hours the residual strength for mix M1 reduces to 92% for 2 hours up to 78% for six hours duration of exposure, for M2 mix 90% for 2 hours duration of exposure up to 76% for six hour duration of exposure, for M3 mix 88% up to 68% between 2 and 6 hours of duration of exposure.5. IMPACT STRENGTH OF CONCRETE5.1 RESIDUAL IMPACT STRENGTH VS TEMPERATUREFrom the table 1, it can be observed that for the sustained elevated temperature of 100°C the residual impact strength of all the specimens reduces and vary between 20 and 50% for mix M1, 15 to 40% for mix M2 and M3. When the sustained elevated temperature is 200°C the residual impact strength of all the mixes further decreases. The reduction is around 60-70% for mix M1, 55 to 65% for M2 and M3 mix. When the sustained elevated temperature is 300°C it is observed that the residual impact strength reduces further and vary between 85 and 70% for mix M1 and 85 to 90% for mix M2 and mix M3.5.2 RESIDUAL IMPACT STRENGTH VS DURATION OF EXPOSUREFrom the Table 1 and Figures 1 to 3, it can be observed that there is a reduction in impact strength when the sustained elevated temperature is 100°C for 2 hrs, 4 hrs and 6 hrs, and its range is 15 to 50% for all the mixes M1, M2 and M3. The influence of duration of exposure is higher for mix M1 which decreases more rapidly as compared to mix M2 and mix M3 for the same duration of exposure. When the specimens are subjected to sustained elevated temperature of 200°C for 2,4 and 6 hour of duration, further reduction in residual impact strength is observed as compared to at 100°C. The reduction is in the range of 55-70% for all the mixes. The six hour duration of exposure has a greater influence on the residual impact strength of concrete. When the sustained elevated temperature is 300°C for 2,4 and 6 hours duration of exposure the residualimpact strength reduces. It can be seen that both temperature and duration of exposure have a very high influence on the residual impact strength of concrete which shows a reduction up to 90% approximately for all the mixes.6. CONCLUSIONThe compressive strength of concrete increases at 100oC when exposed to sustained elevated temperature. The compressive strength of concrete decreases when exposed to 200°C and 300°C from 10 to 30% for 6 hours of exposure. Residual impact strength reduces irrespective of temperature and duration. Residual impact strength decreases at a higher rate of 20% to 85% as compared to compressive strength between 15% and 30 % when subjected to sustained elevated temperature. The impact strength reduces at a higher rate as compared to compressive strength when subjected to sustained elevated temperature.混凝土受持续高温影响的强度的研究混凝土具有显着的耐火性能。

土木工程专业英语课文_翻译_考试必备

土木工程专业英语课文_翻译_考试必备

土木工程专业英语课文_翻译_考试必备土木工程专业英语课文翻译The principal construction materials of earlier times were wood and masonry brick, stone, or tile, and similar materials. The courses or layers were bound together with mortar or bitumen, a tar like substance, or some other binding agent. The Greeks and Romanssometimes used iron rods or claps to strengthen their building. The columns of the Parthenon in Athens, for example, have holes drilled in them for iron bars that have now rusted away. The Romans also used a natural cement called puzzling, made from volcanic ash, that became as hard as stone under water.早期时代的主要施工材料,木材和砌体砖,石,或瓷砖,和类似的材料。

这些课程或层密切联系在一起,用砂浆或沥青,焦油一个样物质,或其他一些有约束力的代理人。

希腊人和罗马人有时用铁棍或拍手以加强其建设。

在雅典的帕台农神庙列,例如,在他们的铁钻的酒吧现在已经生锈了孔。

罗马人还使用了天然水泥称为令人费解的,由火山灰制成,变得像石头一样坚硬在水中。

Both steel and cement, the two most important construction materials of modern times, were introduced in the nineteenth century. Steel, basically an alloy of iron and a small amount of carbon had been made up to that time by a laborious process that restricted it to such special uses as sword blades. After the invention of the Bessemer process in 1856, steel was available in large quantities at low prices. The enormous advantage of steel is its tensile force which, as we have seen,tends to pull apart many materials. New alloys have further, which is a tendency for it to weaken as a result of continual changes in stress.钢铁和水泥,两个最重要的现代建筑材料,介绍了在十九世纪。

土木工程英语文献原文及中文翻译

土木工程英语文献原文及中文翻译

Civil engineering introduction papers[英语原文]Abstract: the civil engineering is a huge discipline, but the main one is building, building whether in China or abroad, has a long history, long-term development process. The world is changing every day, but the building also along with the progress of science and development. Mechanics findings, material of update, ever more scientific technology into the building. But before a room with a tile to cover the top of the house, now for comfort, different ideas, different scientific, promoted the development of civil engineering, making it more perfect.[key words] : civil engineering; Architecture; Mechanics, Materials.Civil engineering is build various projects collectively. It was meant to be and "military project" corresponding. In English the history of Civil Engineering, mechanical Engineering, electrical Engineering, chemical Engineering belong to to Engineering, because they all have MinYongXing. Later, as the project development of science and technology, mechanical, electrical, chemical has gradually formed independent scientific, to Engineering became Civil Engineering of specialized nouns. So far, in English, to Engineering include water conservancy project, port Engineering, While in our country, water conservancy projects and port projects also become very close and civil engineering relatively independent branch. Civil engineering construction of object, both refers to that built on the ground, underground water engineering facilities, also refers to applied materials equipment and conduct of the investigation, design and construction, maintenance, repair and other professional technology.Civil engineering is a kind of with people's food, clothing, shelter and transportation has close relation of the project. Among them with "live" relationship is directly. Because, to solve the "live" problem must build various types of buildings. To solve the "line, food and clothes" problem both direct side, but also a indirect side. "Line", must build railways, roads, Bridges, "Feed", must be well drilling water, water conservancy, farm irrigation, drainage water supply for the city, that is direct relation. Indirectly relationship is no matter what you do, manufacturing cars, ships, or spinning and weaving, clothing, or even production steel, launch satellites, conducting scientific research activities are inseparable from build various buildings, structures and build all kinds of project facilities.Civil engineering with the progress of human society and development, yet has evolved into large-scale comprehensive discipline, it has out many branch, such as: architectural engineering, the railway engineering, road engineering, bridge engineering, special engineering structure, waterand wastewater engineering, port engineering, hydraulic engineering, environment engineering disciplines. [1]Civil engineering as an important basic disciplines, and has its important attributes of: integrated, sociality, practicality, unity. Civil engineering for the development of national economy and the improvement of people's life provides an important material and technical basis, for many industrial invigoration played a role in promoting, engineering construction is the formation of a fixed asset basic production process, therefore, construction and real estate become in many countries and regions, economic powerhouses.Construction project is housing planning, survey, design, construction of the floorboard. Purpose is for human life and production provide places.Houses will be like a man, it's like a man's life planning environment is responsible by the planners, Its layout and artistic processing, corresponding to the body shape looks and temperament, is responsible by the architect, Its structure is like a person's bones and life expectancy, the structural engineer is responsible, Its water, heating ventilation and electrical facilities such as the human organ and the nerve, is by the equipment engineer is responsible for. Also like nature intact shaped like people, in the city I district planning based on build houses, and is the construction unit, reconnaissance unit, design unit of various design engineers and construction units comprehensive coordination and cooperation process.After all, but is structural stress body reaction force and the internal stress and how external force balance. Building to tackle, also must solve the problem is mechanical problems. We have to solve the problem of discipline called architectural mechanics. Architectural mechanics have can be divided into: statics, material mechanics and structural mechanics three mechanical system. Architectural mechanics is discussion and research building structure and component in load and other factors affecting the working condition of, also is the building of intensity, stiffness and stability. In load, bear load and load of structure and component can cause the surrounding objects in their function, and the object itself by the load effect and deformation, and there is the possibility of damage, but the structure itself has certain resistance to deformation and destruction of competence, and the bearing capacity of the structure size is and component of materials, cross section, and the structural properties of geometry size, working conditions and structure circumstance relevant. While these relationships can be improved by mechanics formula solved through calculation.Building materials in building and has a pivotal role. Building material is with human society productivity and science and technologyimproves gradually developed. In ancient times, the human lives, the line USES is the rocks andTrees. The 4th century BC, 12 ~ has created a tile and brick, humans are only useful synthetic materials made of housing. The 17th century had cast iron and ShouTie later, until the eighteenth century had Portland cement, just make later reinforced concrete engineering get vigorous development. Now all sorts of high-strength structural materials, new decoration materials and waterproof material development, criterion and 20th century since mid organic polymer materials in civil engineering are closely related to the widely application. In all materials, the most main and most popular is steel, concrete, lumber, masonry. In recent years, by using two kinds of material advantage, will make them together, the combination of structure was developed. Now, architecture, engineering quality fit and unfit quality usually adopted materials quality, performance and using reasonable or not have direct connection, in meet the same technical indicators and quality requirements, under the precondition of choice of different material is different, use method of engineering cost has direct impact.In construction process, building construction is and architectural mechanics, building materials also important links. Construction is to the mind of the designer, intention and idea into realistic process, from the ancient hole JuChao place to now skyscrapers, from rural to urban country road elevated road all need through "construction" means. A construction project, including many jobs such as dredging engineering, deep foundation pit bracing engineering, foundation engineering, reinforced concrete structure engineering, structural lifting project, waterproofing, decorate projects, each type of project has its own rules, all need according to different construction object and construction environment conditions using relevant construction technology, in work-site.whenever while, need and the relevant hydropower and other equipment composition of a whole, each project between reasonable organizing and coordination, better play investment benefit. Civil engineering construction in the benefit, while also issued by the state in strict accordance with the relevant construction technology standard, thus further enhance China's construction level to ensure construction quality, reduce the cost for the project.Any building built on the surface of the earth all strata, building weight eventually to stratum, have to bear. Formation Support building the rocks were referred to as foundation, and the buildings on the ground and under the upper structure of self-respect and liable to load transfer to the foundation of components or component called foundation. Foundation, and the foundation and the superstructure is a building of three inseparable part. According to the function is different, but in load, under the action of them are related to each other, is theinteraction of the whole. Foundation can be divided into natural foundation and artificial foundation, basic according to the buried depth is divided into deep foundation and shallow foundation. , foundation and foundation is the guarantee of the quality of the buildings and normal use close button, where buildings foundation in building under loads of both must maintain overall stability and if the settlement of foundation produce in building scope permitted inside, and foundation itself should have sufficient strength, stiffness and durability, also consider repair methods and the necessary foundation soil retaining retaining water and relevant measures. [3]As people living standard rise ceaselessly, the people to their place of building space has become not only from the number, and put forward higher requirement from quality are put car higher demands that the environment is beautiful, have certain comfort. This needs to decorate a building to be necessary. If architecture major engineering constitutes the skeleton of the building, then after adornment building has become the flesh-and-blood organism, final with rich, perfect appearance in people's in front, the best architecture should fully embody all sorts of adornment material related properties, with existing construction technology, the most effective gimmick, to achieve conception must express effect. Building outfit fix to consider the architectural space use requirement, protect the subject institutions from damage, give a person with beautifulenjoying, satisfy the requirements of fire evacuation, decorative materials and scheme of rationality, construction technology and economic feasibility, etc. Housing construction development and at the same time, like housing construction as affecting people life of roads, Bridges, tunnels has made great progress.In general civil engineering is one of the oldest subjects, it has made great achievements, the future of the civil engineering will occupy in people's life more important position. The environment worsening population increase, people to fight for survival, to strive for a more comfortable living environment, and will pay more attention to civil engineering. In the near future, some major projects extimated to build, insert roller skyscrapers, across the oceanBridges, more convenient traffic would not dream. The development of science and technology, and the earth is deteriorating environment will be prompted civil engineering to aerospace and Marine development, provide mankind broader space of living. In recent years, engineering materials mainly is reinforced concrete, lumber and brick materials, in the future, the traditional materials will be improved, more suitable for some new building materials market, especially the chemistry materials will promote the construction of towards a higher point. Meanwhile, design method of precision, design work of automation, information and intelligent technology of introducing, will be people have a morecomfortable living environment. The word, and the development of the theory and new materials, the emergence of the application of computer, high-tech introduction to wait to will make civil engineering have a new leap.This is a door needs calm and a great deal of patience and attentive professional. Because hundreds of thousands, even hundreds of thousands of lines to building each place structure clearly reflected. Without a gentle state of mind, do what thing just floating on the surface, to any a building structure, to be engaged in business and could not have had a clear, accurate and profound understanding of, the nature is no good. In this business, probably not burn the midnight oil of courage, not to reach the goal of spirit not to give up, will only be companies eliminated.This is a responsible and caring industry. Should have a single responsible heart - I one's life in my hand, thousands of life in my hand. Since the civil, should choose dependably shoulder the responsibility.Finally, this is a constant pursuit of perfect industry. Pyramid, spectacular now: The Great Wall, the majestic... But if no generations of the pursuit of today, we may also use the sort of the oldest way to build this same architecture. Design a building structure is numerous, but this is all experienced centuries of clarification, through continuous accumulation, keep improving, innovation obtained. And such pursuit, not confined in the past. Just think, if the design of a building can be like calculation one plus one equals two as simple and easy to grasp, that was not for what? Therefore, a civil engineer is in constant of in formation. One of the most simple structure, the least cost, the biggest function. Choose civil, choosing a steadfast diligence, innovation, pursuit of perfect path.Reference:[1] LuoFuWu editor. Civil engineering (professional). Introduction to wuhan. Wuhan university of technology press. 2007[2] WangFuChuan, palace rice expensive editor. Construction engineering materials. Beijing. Science and technology literature press. 2002[3] jiang see whales, zhiming editor. Civil engineering introduction of higher education press. Beijing.. 1992土木工程概论 [译文]摘要:土木工程是个庞大的学科,但最主要的是建筑,建筑无论是在中国还是在国外,都有着悠久的历史,长期的发展历程。

土木工程建筑外文文献及翻译

土木工程建筑外文文献及翻译

土木工程建筑外文文献及翻译土木工程建筑外文文献及翻译Cyclic behavior of steel moment frame connections under varying axial load and lateral displacementsAbstractThis paper discusses the cyclic behavior of four steel moment connections tested under variable axial load and lateral displacements. The beam specim- ens consisted of a reducedbeam section, wing plates and longitudinal stiffeners. The test specimens were subjected to varying axial forces and lateral displace- ments to simulate the effects on beams in a Coupled-Girder Moment-Resisting Framing system under lateral loading. The test results showed that the specim- ens responded in a ductile manner since the plastic rotations exceeded 0.03 rad without significant drop in the lateral capacity. The presence of the longitudin- al stiffener assisted in transferring the axial forces and delayed the formation of web local buckling.1. IntroductionAimed at evaluating the structural performance of reduced-beam section(RBS) connections under alternated axial loading and lateral displacement, four full-scale specimens were tested. These tests were intended to assess the performance of the moment connection design for the Moscone Center Exp- ansion under the Design Basis Earthquake (DBE) and the Maximum Considered Earthquake (MCE). Previous research conducted on RBS moment connections [1,2] showed that connections with RBS profiles can achieve rotations in excess of 0.03 rad. However, doubts have been cast on the quality of the seismic performance of theseconnections under combined axial and lateral loading.The Moscone Center Expansion is a three-story, 71,814 m2 (773,000 ft2) structure with steel moment frames as its primary lateral force-resisting system. A three dimensional perspective illustration is shown in Fig. 1. The overall height of the building, at the highest point of the exhibition roof, is approxima- tely 35.36 m (116ft) above ground level. The ceiling height at the exhibition hall is 8.23 m (27 ft) , and the typical floor-to-floor height in the building is 11.43 m (37.5 ft). The building was designed as type I according to the requi- rements of the 1997 Uniform Building Code. The framing system consists of four moment frames in the East–West direct- ion, one on either side of the stair towers, and four frames in the North–South direction, one on either side of the stair and elevator cores in the east end and two at the west end of the structure [4]. Because of the story height, the con- cept of the Coupled-Girder Moment-Resisting Framing System (CGMRFS) was utilized.By coupling the girders, the lateral load-resisting behavior of the moment framing system changes to one where structural overturning moments are resisted partially by an axial compression–tension couple across the girder system, rather than only by the individual flexural action of the girders. As a result, a stiffer lateral load resisting system is achieved. The vertical element that connects the girders is referred to as a coupling link. Coupling links are analogous to and serve the same structural role as link beams in eccentrically braced frames. Coupling links are generally quite short, having a large shear- to-moment ratio.Under earthquake-type loading, the CGMRFS subjects its girders to wariab- ble axial forces in addition to their endmoments. The axial forces in theFig. 1. Moscone Center Expansion Project in San Francisco, CAgirders result from the accumulated shear in the link.2. Analytical model of CGMRFNonlinear static pushover analysis was conducted on a typical one-bay model of the CGMRF. Fig. 2 shows the dimensions and the various sections of the 10 in) and the ?254 mm (1 1/8 in ?model. The link flange plates were 28.5 mm 18 3/4 in). The SAP 2000 computer ?476 mm (3 /8 in ?web plate was 9.5 mm program was utilized in the pushover analysis [5]. The frame was characterized as fully restrained(FR). FR moment frames are those frames for 1170 which no more than 5% of the lateral deflections arise from connection deformation [6]. The 5% value refers only to deflection due to beam–column deformation and not to frame deflections that result from column panel zone deformation [6, 9].The analysis was performed using an expected value of the yield stress and ultimate strength. These values were equal to 372 MPa (54 ksi) and 518 MPa (75 ksi), respective ly. The plastic hinges’ load–deformation behavior was approximated by the generalized curve suggested by NEHRP Guidelines for the Seismic Rehab ilitation of Buildings [6] as shown in Fig. 3. △y was calcu- lated based on Eqs. (5.1) and (5.2) from [6], as follows: P–M hinge load–deformation model points C, D and E are based on Table 5.4 from [6] for△y was taken as 0.01 rad per Note 3 in [6], Table 5.8. Shear hinge load- load–deformation model points C, D and E are based on Table 5.8 [6], Link Beam, Item a. A strain hardening slope between points B and C of 3% of the elastic slope was assumedfor both models.The following relationship was used to account for moment–axial load interaction [6]:where MCE is the expected moment strength, ZRBS is the RBS plastic section modulus (in3), is the expected yield strength of the material (ksi), P is the axial force in the girder (kips) and is the expected axial yield force of the RBS, equal to (kips). The ultimate flexural capacities of the beam and the link of the model are shown in Table 1.Fig. 4 shows qualitatively the distribution of the bending moment, shear force, and axial force in the CGMRF under lateral load. The shear and axial force in the beams are less significant to the response of the beams as compared with the bending moment, although they must be considered in design. The qualita- tive distribution of internal forces illustrated in Fig. 5 is fundamentally the same for both elastic and inelastic ranges of behavior. The specific values of the internal forces will change as elements of the frame yield and internal for- ces are redistributed. The basic patterns illustrated in Fig. 5, however, remain the same.Inelastic static pushover analysis was carried out by applying monotonically increasing lateral displacements, at the top of both columns, as shown in Fig. 6. After the four RBS have yielded simultaneously, a uniform yielding in the web and at the ends of the flanges of the vertical link will form. This is the yield mechanism for the frame , with plastic hinges also forming at the base of the columns if they are fixed. The base shear versus drift angle of the model is shown in Fig. 7 . The sequence of inelastic activity in the frame is shown on the figure. An elastic component, a long transition (consequence of the beam plastic hinges being formed simultaneously) and a narrow yield plateaucharacterize the pushover curve.The plastic rotation capacity, qp, is defined as the total plastic rotation beyond which the connection strength starts to degrade below 80% [7]. This definition is different from that outlined in Section 9 (Appendix S) of the AISC Seismic Provisions [8, 10]. Using Eq. (2) derived by Uang and Fan [7], an estimate of the RBS plastic rotation capacity was found to be 0.037 rad:Fyf was substituted for Ry?Fy [8], where Ry is used to account for the differ- ence between the nominal and the expected yield strengths (Grade 50 steel, Fy=345 MPa and Ry =1.1 are used).3. Experimental programThe experimental set-up for studying the behavior of a connection was based on Fig. 6(a). Using the plastic displacement dp, plastic rotation gp, and plastic story drift angle qp shown in the figure, from geometry, it follows that:And:in which d and g include the elastic components. Approximations as above are used for large inelastic beam deformations. The diagram in Fig. 6(a) suggest that a sub assemblage with displacements controlled in the manner shown in Fig. 6(b) can represent the inelastic behavior of a typical beam in a CGMRF.The test set-up shown in Fig. 8 was constructed to develop the mechanism shown in Fig. 6(a) and (b). The axial actuators were attached to three 2438 mm × 1219 mm ×1219 mm (8 ft × 4 ft × 4 ft) RC blocks. These blocks were tensioned to the laboratory floor by means of twenty-four 32 mm diameter dywidag rods. This arrangement permitted replacement of the specimen after each test.Therefore, the force applied by the axial actuator, P, can beresolved into two or thogonal components, Paxial and Plateral. Since the inclination angle of the axial actuator does not exceed , therefore Paxial is approximately equal to P [4]. However, the lateral 3.0 component, Plateral, causes an additional moment at the beam-to column joint. If the axial actuators compress the specimen, then the lateral components will be adding to the lateral actuator forces, while if the axial actuators pull the specimen, the Plateral will be an opposing force to the lateral actuators. When the axial actuators undergoaxial actuators undergo a lateral displacement _, they cause an additional moment at the beam-to-column joint (P-△effect). Therefore, the moment at the beam-to column joint is equal to: where H is the lateral forces, L is the arm, P is the axial force and _ is the lateral displacement.Four full-scale experiments of beam column connections were conducted.The member sizes and the results of tensile coupon tests are listed in Table 2All of the columns and beams were of A572 Grade 50 steel (Fy 344.5 MPa). The actual measured beam flange yield stress value was equal to 372 MPa (54 ksi), while the ultimate strength ranged from 502 MPa (72.8 ksi) to 543 MPa (78.7 ksi).Table 3 shows the values of the plastic moment for each specimen (based on measured tensile coupon data) at the full cross-section and at the reduced section at mid-length of the RBS cutout.The specimens were designated as specimen 1 through specimen 4. Test specimens details are shown in Fig. 9 through Fig. 12. The following features were utilized in the design of the beam–column connection:The use of RBS in beam flanges. A circular cutout was provided, as illustr- ated in Figs. 11 and 12. For all specimens, 30% of the beam flange width was removed. The cuts were made carefully, and then ground smooth in a direct- tion parallel to the beam flange to minimize notches.Use of a fully welded web connection. The connection between the beam web and the column flange was made with a complete joint penetration groove weld (CJP). All CJP welds were performed according to AWS D1.1 Structural Welding Code Use of two side plates welded with CJP to exterior sides of top and bottom beam flan- ges, from the face of the column flange to the beginning of the RBS, as shown in Figs. 11 and 12. The end of the side plate was smoothed to meet the beginning of the RBS. The side plates were welded with CJP with the column flanges. The side plate was added to increase the flexural capacity at the joint location, while the smooth transition was to reduce the stress raisers, which may initiate fractureTwo longitudinal stiffeners, 95 mm × 35 mm (3 3/4 in × 1 3/8 in), were welded with 12.7 mm (1/2 in) fillet weld at the middle height of the web as shown in Figs. 9 and 10. The stiffeners were welded with CJP to column flanges.Removal of weld tabs at both the top and bottom beam flange groove welds. The weld tabs were removed to eliminate any potential notches introduced by the tabs or by weld discontinuities in the groove weld run out regionsUse of continuity plates with a thickness approximately equal to the beam flange thickness. One-inch thick continuity plates were used for all specimens.While the RBS is the most distinguishing feature of these test specimens, the longitudinal stiffener played an important role indelaying the formation of web local buckling and developing reliable connection4. Loading historySpecimens were tested by applying cycles of alternated load with tip displacement increments of _y as shown in Table 4. The tip displacement of the beam was imposed by servo-controlled actuators 3 and 4. When the axial force was to be applied, actuators 1 and 2 were activated such that its force simulates the shear force in the link to be transferred to the beam. 0.5_y. After The variable axial force was increased up to 2800 kN (630 kip) at that, this lo- ad was maintained constant through the maximum lateral displacement.maximum lateral displacement. As the specimen was pushed back the axialforce remained constant until 0.5 y and then started to decrease to zero as the specimen passed through the neutral position [4]. According to the upper bound for beam axial force as discussed in Section 2 of this paper, it was concluded that P =2800 kN (630 kip) is appropriate to investigate this case in RBS loading. The tests were continued until failure of the specimen, or until limitations of the test set-up were reached.5. Test resultsThe hysteretic response of each specimen is shown in Fig. 13 and Fig. 16. These plots show beam moment versus plastic rotation. The beam moment is measured at the middle of the RBS, and was computed by taking an equiva- lent beam-tip force multiplied by the distance between the centerline of the lateral actuator to the middle of the RBS (1792 mm for specimens 1 and 2, 3972 mm for specimens 3 and 4). The equivalent lateral force accounts for the additional moment due to P–△effect. Therotation angle was defined as the lateral displacement of the actuator divided by the length between the centerline of the lateral actuator to the mid length of the RBS. The plastic rotation was computed as follows [4]:where V is the shear force, Ke is the ratio of V/q in the elastic range. Measurements and observations made during the tests indicated that all of the plastic rotation in specimen 1 to specimen 4 was developed within the beam. The connection panel zone and the column remained elastic as intended by design.5.1. Specimens 1 and 2The responses of specimens 1 and 2 are shown in Fig. 13. Initial yielding occurred during cycles 7 and 8 at 1_y with yielding observed in the bottom flange. For all test specimens, initial yielding was observed at this location and attributed to the moment at the base of the specimen [4]. Progressing through the loading history, yielding started to propagate along the RBS bottom flange. During cycle 3.5_y initiation of web buckling was noted adjacent to the yielded bottom flange. Yielding started to propagate along the top flange of the RBS and some minor yielding along the middle stiffener. During the cycle of 5_y with the increased axial compression load to 3115 KN (700 kips) a severe web buckle developed along with flange local buckling. The flange and the web local buckling became more pronounced with each successive loading cycle. It should be noted here that the bottom flange and web local buckling was not accompanied by a significant deterioration in the hysteresis loops.A crack developed in specimen 1 bottom flange at the end of the RBS where it meets the side plate during the cycle 5.75_y. Upon progressing through the loading history, 7_y, the crackspread rapidly across the entire width of the bottom flange. Once the bottom flange was completely fractured, the web began to fracture. This fracture appeared to initiate at the end of the RBS,then propagated through the web net section of the shear tab, through the middle stiffener and the through the web net section on the other side of the stiffener. The maximum bending moment achieved on specimen 1 during theDuring the cycle 6.5 y, specimen 2 also showed a crack in the bottom flange at the end of the RBS where it meets the wing plate. Upon progressing thou- gh the loading history, 15 y, the crack spread slowly across the bottom flan- ge. Specimen 2 test was stopped at this point because the limitation of the test set-up was reached.The maximum force applied to specimens 1 and 2 was 890 kN (200 kip). The kink that is seen in the positive quadrant is due to the application of the varying axial tension force. The load-carrying capacity in this zone did not deteriorate as evidenced with the positive slope of the force–displacement curve. However, the load-carrying capacity deteriorated slightly in the neg- ative zone due to the web and the flange local buckling.Photographs of specimen 1 during the test are shown in Figs.14 and 15. Severe local buckling occurred in the bottom flange and portion of the web next to the bottom flange as shown in Fig. 14. The length of this buckle extended over the entire length of the RBS. Plastic hinges developed in the RBS with extensive yielding occurring in the beam flanges as well as the web. Fig. 15 shows the crack that initiated along the transition of the RBS to the side wing plate. Ultimate fracture of specimen 1 was caused by a fracture in the bottom flange. This fracture resulted in almost total loss of the beam- carrying capacity. Specimen 1 developed0.05 rad of plastic rotation and showed no sign of distress at the face of the column as shown in Fig. 15.5.2. Specimens 3 and 4The response of specimens 3 and 4 is shown in Fig. 16. Initial yielding occured during cycles 7 and 8 at 1_y with significant yielding observed in the bottom flange. Progressing through the loading history, yielding started to propagate along the bottom flange on the RBS. During cycle 1.5_y initiation of web buckling was noted adjacent to the yielded bottom flange. Yielding started to propagate along the top flange of the RBS and some minor yielding along the middle stiffener. During the cycle of 3.5_y a severe web buckle developed along with flange local buckling. The flange and the web local buckling bec- ame more pronounced with each successive loading cycle.During the cycle 4.5 y, the axial load was increased to 3115 KN (700 kips) causing yielding to propagate to middle transverse stiffener. Progressing through the loading history, the flange and the web local buckling became more severe. For both specimens, testing was stopped at this point due to limitations in the test set-up. No failures occurred in specimens 3 and 4. However, upon removing specimen 3 to outside the laboratory a hairline crack was observed at the CJP weld of the bottom flange to the column.The maximum forces applied to specimens 3 and 4 were 890 kN (200 kip) and 912 kN (205 kip). The load-carrying capacity deteriorated by 20% at the end of the tests for negative cycles due to the web and the flange local buckling. This gradual reduction started after about 0.015 to 0.02 rad of plastic rotation. The load-carrying capacity during positive cycles (axial tension applied in the girder) did not deteriorate as evidenced with the slope of the force–displacement envelope for specimen 3 shownin Fig. 17.A photograph of specimen 3 before testing is shown in Fig.18. Fig. 19 is aFig. 16. Hysteretic behavior of specimens 3 and 4 in terms of moment at middle RBS versus beam plastic rotation.photograph of specimen 4 taken after the application of 0.014 rad displacem- ent cycles, showing yielding and local buckling at the hinge region. The beam web yielded over its full depth. The most intense yielding was observed in the web bottom portion, between the bottom flange and the middle stiffener. The web top portion also showed yielding, although less severe than within the bottom portion. Yielding was observed in the longitudinal stiffener. No yiel- ding was observed in the web of the column in the joint panel zone. The un- reduced portion of the beam flanges near the face of the column did not show yielding either. The maximum displacement applied was 174 mm, and the maximum moment at the middle of the RBS was 1.51 times the plastic mom ent capacity of the beam. The plastic hinge rotation reached was about 0.032 rad (the hinge is located at a distance 0.54d from the column surface,where d is the depth of the beam).5.2.1. Strain distribution around connectionThe strain distribution across the flanges–outer surface of specimen 3 is shown in Figs. 20 and 21. The readings and the distributions of the strains in specimens 1, 2 and 4 (not presented) showed a similar trend. Also the seque- nce of yielding in these specimens is similar to specimen 3.The strain at 51 mm from the column in the top flange–outer surface remained below 0.2% during negative cycles. The top flange, at the same location, yielded in compression only Thelongitudinal strains along the centerline of the bottom–flange outer face are shown in Figs. 22 and 23 for positive and negative cycles, respectively. From Fig.23, it is found that the strain on the RBS becomes several times larg- er than that near the column after cycles at –1.5_y; this is responsible for theflange local buckling. Bottom flange local buckling occurred when the average strain in the plate reached the strain-hardening value (esh _ 0.018) and the reduced-beam portion of the plate was fully yielded under longitudinal stresses and permitted the development of a full buckled wave.5.2.2. Cumulative energy dissipatedThe cumulative energy dissipated by the specimens is shown in Fig. 24. The cumulative energy dissipated was calculated as the sum of the areas enclosed the lateral load–lateral displacement hysteresis loops. Energy dissipation sta- rted to increase after cycle 12 at 2.5 y (Fig. 19). At large drift levels, energy dissipation augments significantly with small changes in drift. Specimen 2 dissipated more energy than specimen 1, which fractured at RBS transition. However, for both specimens the trend is similar up to cycles at q =0.04 radIn general, the dissipated energy during negative cycles was1.55 times bigger than that for positive cycles in specimens 1 and2. For specimens 3 and 4 the dissipated energy during negative cycles was 120%, on the average, that of the positive cycles. The combined phenomena of yielding, strain hardening, in-plane and out- of-plane deformations, and local distortion all occurred soon after the bottom flange RBS yielded.6. ConclusionsBased on the observations made during the tests, and on the analysis of the instrumentation, the following conclusions weredeveloped:1. The plastic rotation exceeded the 3% radians in all test specimens.2. Plastification of RBS developed in a stable manner.3. The overstrength ratios for the flexural strength of the test specimens were equal to 1.56 for specimen 1 and 1.51 for specimen4. The flexural strength capacity was based on the nominal yield strength and on the FEMA-273 beam–column equation.4. The plastic local buckling of the bottom flange and the web was not accompanied by a significant deterioration in the load-carrying capacity.5. Although flange local buckling did not cause an immediate degradation of strength, it did induce web local buckling.6. The longitudinal stiffener added in the middle of the beam web assisted in transferring the axial forces and in delaying the formation of web local buckling. How ever, this has caused a much higher overstrength ratio, which had a significant impact on the capacity design of the welded joints, panel zone and the column.7. A gradual strength reduction occurred after 0.015 to 0.02 rad of plastic rotation during negative cycles. No strength degradation was observed during positive cycles.8. Compression axial load under 0.0325Py does not affect substantially the connection deformation capacity.9. CGMRFS with properly designed and detailed RBS connections is a reliable system to resist earthquakes.AcknowledgementsStructural Design Engineers, Inc. of San Francisco financially supported the experimental program. The tests were performedin the Large Scale Structures Laboratory of the University of Nevada, Reno. The participation of Elizabeth Ware, Adrianne Dietrich and of the technical staff is gratefully acknowledged.References受弯钢框架结点在变化轴向荷载和侧向位移的作用下的周期性行为摘要这篇论文讨论的是在变化的轴向荷载和侧向位移的作用下,接受测试的四种受弯钢结点的周期性行为。

土木工程毕业设计外文翻译最终中英文

土木工程毕业设计外文翻译最终中英文

7 Rigid-Frame StructuresA rigid-frame high-rise structure typically comprises parallel or orthogonally arranged bents consisting of columns and girders with moment resistant joints. Resistance to horizontal loading is provided by the bending resistance of the columns, girders, and joints. The continuity of the frame also contributes to resisting gravity loading, by reducing the moments in the girders.The advantages of a rigid frame are the simplicity and convenience of its rectangular form.Its unobstructed arrangement, clear of bracing members and structural walls, allows freedom internally for the layout and externally for the fenestration. Rigid frames are considered economical for buildings of up to' about25 stories, above which their drift resistance is costly to control. If, however,a rigid frame is combined with shear walls or cores, the resulting structure is very much stiffer so that its height potential may extend up to 50 stories or more. A flat plate structure is very similar to a rigid frame, but with slabs replacing the girders As with a rigid frame, horizontal and vertical loadings are resisted in a flat plate structure by the flexural continuity between the vertical and horizontal components.As highly redundant structures, rigid frames are designed initially on the basis of approximate analyses, after which more rigorous analyses and checks can be made. The procedure may typically include the following stages:1. Estimation of gravity load forces in girders and columns by approximate method.2. Preliminary estimate of member sizes based on gravity load forces witharbitrary increase in sizes to allow for horizontal loading.3. Approximate allocation of horizontal loading to bents and preliminary analysisof member forces in bents.4. Check on drift and adjustment of member sizes if necessary.5. Check on strength of members for worst combination of gravity and horizontalloading, and adjustment of member sizes if necessary.6. Computer analysis of total structure for more accurate check on memberstrengths and drift, with further adjustment of sizes where required. This stage may include the second-order P-Delta effects of gravity loading on the member forces and drift..7. Detailed design of members and connections.This chapter considers methods of analysis for the deflections and forces for both gravity and horizontal loading. The methods are included in roughly the order of the design procedure, with approximate methods initially and computer techniques later. Stability analyses of rigid frames are discussed in Chapter 16.7.1 RIGID FRAME BEHAVIORThe horizontal stiffness of a rigid frame is governed mainly by the bending resistance of the girders, the columns, and their connections, and, in a tall frame, by the axial rigidity of the columns. The accumulated horizontal shear above any story of a rigid frame is resisted by shear in the columns of that story (Fig. 7.1). The shear causes the story-height columns to bend in double curvature with points of contraflexure at approximately mid-story-height levels. The moments applied to a joint from the columns above and below are resisted by the attached girders, which also bend in double curvature, with points of contraflexure at approximately mid-span. These deformations of the columns and girders allow racking of the frame and horizontal deflection in each story. The overall deflected shape of a rigid frame structure due to racking has a shear configuration with concavity upwind, a maximum inclination near the base, and a minimum inclination at the top, as shown in Fig.7.1.The overall moment of the external horizontal load is resisted in each story level by the couple resulting from the axial tensile and compressive forces in the columns on opposite sides of the structure (Fig. 7.2). The extension and shortening of the columns cause overall bending and associated horizontal displacements of the structure. Because of the cumulative rotation up the height, the story drift dueto overall bending increases with height, while that due to racking tends to decrease. Consequently the contribution to story drift from overall bending may, in. the uppermost stories, exceed that from racking. The contribution of overall bending to the total drift, however, will usually not exceed 10% of that of racking, except in very tall, slender,, rigid frames. Therefore the overall deflected shape of a high-rise rigid frame usually has a shear configuration.The response of a rigid frame to gravity loading differs from a simply connected frame in the continuous behavior of the girders. Negative moments are induced adjacent to the columns, and positive moments of usually lesser magnitude occur in the mid-span regions. The continuity also causes the maximum girder moments to be sensitive to the pattern of live loading. This must be considered when estimating the worst moment conditions. For example, the gravity load maximum hogging moment adjacent to an edge column occurs when live load acts only on the edge span and alternate other spans, as for A in Fig. 7.3a. The maximum hogging moments adjacent to an interior column are caused, however, when live load acts only on the spans adjacent to the column, as for B in Fig. 7.3b. The maximum mid-span sagging moment occurs when live load acts on the span under consideration, and alternate other spans, as for spans AB and CD in Fig. 7.3a.The dependence of a rigid frame on the moment capacity of the columns for resisting horizontal loading usually causes the columns of a rigid frame to be larger than those of the corresponding fully braced simply connected frame. On the other hand, while girders in braced frames are designed for their mid-span sagging moment, girders in rigid frames are designed for the end-of-span resultant hogging moments, which may be of lesser value. Consequently, girders in a rigid frame may be smaller than in the corresponding braced frame. Such reductions in size allow economy through the lower cost of the girders and possible reductions in story heights. These benefits may be offset, however, by the higher cost of the more complex rigid connections.7.2 APPROXIMATE DETERMINATION OF MEMBER FORCES CAUSED BY GRAVITY LOADSIMGA rigid frame is a highly redundant structure; consequently, an accurate analysis can be made only after the member sizes are assigned. Initially, therefore, member sizes are decided on the basis of approximate forces estimated either by conservative formulas or by simplified methods of analysis that are independent of member properties. Two approaches for estimating girder forces due to gravity loading are given here.7.2.1 Girder Forces—Code Recommended ValuesIn rigid frames with two or more spans in which the longer of any two adjacent spans does not exceed the shorter by more than 20 %, and where the uniformly distributed design live load does not exceed three times the dead load, the girder moment and shears may be estimated from Table 7.1. This summarizes the recommendations given in the Uniform Building Code [7.1]. In other cases a conventional moment distribution or two-cycle moment distribution analysis should be made for a line of girders at a floor level.7.2.2 Two-Cycle Moment Distribution [7.2].This is a concise form of moment distribution for estimating girder moments in a continuous multibay span. It is more accurate than the formulas in Table 7.1, especially for cases of unequal spans and unequal loading in different spans.The following is assumed for the analysis:1. A counterclockwise restraining moment on the end of a girder is positive anda clockwise moment is negative.2. The ends of the columns at the floors above and below the considered girder are fixed.3. In the absence of known member sizes, distribution factors at each joint aretaken equal to 1 /n, where n is the number of members framing into the joint in the plane of the frame.Two-Cycle Moment Distribution—Worked Example. The method is demonstrated by a worked example. In Fig, 7.4, a four-span girder AE from a rigid-frame bent is shown with its loading. The fixed-end moments in each span are calculated for dead loading and total loading using the formulas given in Fig, 7.5. The moments are summarized in Table 7.2.The purpose of the moment distribution is to estimate for each support the maximum girder moments that can occur as a result of dead loading and pattern live loading.A different load combination must be considered for the maximum moment at each support, and a distribution made for each combination.The five distributions are presented separately in Table 7.3, and in a combined form in Table 7.4. Distributions a in Table 7.3 are for the exterior supports A andE. For the maximum hogging moment at A, total loading is applied to span AB with dead loading only on BC. The fixed-end moments are written in rows 1 and 2. In this distribution only .the resulting moment at A is of interest. For the first cycle, joint B is balanced with a correcting moment of- (-867 + 315)/4 = - U/4 assigned to M BA where U is the unbalanced moment. This is not recorded, but half of it, ( - U/4)/2, is carried over to M AB. This is recorded in row 3 and then added to the fixed-end moment and the result recorded in row 4.The second cycle involves the release and balance of joint A. The unbalanced moment of 936 is balanced by adding-U/3 = -936/3 = -312 to M BA (row 5), implicitly adding the same moment to the two column ends at A. This completes the second cycle of the distribution. The resulting maximum moment at A is then given by the addition of rows 4 and 5, 936 - 312 = 624. The distribution for the maximum moment at E follows a similar procedure.Distribution b in Table 7.3 is for the maximum moment at B. The most severe loading pattern for this is with total loading on spans AB and BC and dead load only on CD. The operations are similar to those in Distribution a, except that the T first cycle involves balancing the two adjacent joints A and C while recording only their carryover moments to B. In the second cycle, B is balanced by adding - (-1012 + 782)/4 = 58 to each side of B. The addition of rows 4 and 5 then gives the maximum hogging moments at B. Distributions c and d, for the moments at joints C and D, follow patterns similar to Distribution b.The complete set of operations can be combined as in Table 7.4 by initially recording at each joint the fixed-end moments for both dead and total loading. Then the joint, or joints, adjacent to the one under consideration are balanced for the appropriate combination of loading, and carryover moments assigned .to the considered joint and recorded. The joint is then balanced to complete the distribution for that support.Maximum Mid-Span Moments. The most severe loading condition for a maximum mid-span sagging moment is when the considered span and alternate other spans and total loading. A concise method of obtaining these values may be included in the combined two-cycle distribution, as shown in Table 7.5. Adopting the convention that sagging moments at mid-span are positive, a mid-span total; loading moment is calculated for the fixed-end condition of each span and entered in the mid-span column of row 2. These mid-span moments must now be corrected to allow for rotation of the joints. This is achieved by multiplying the carryover moment, row 3, at the left-hand end of the span by (1 + 0.5 D.F. )/2, and the carryover moment at the right-hand end by -(1 + 0.5 D.F.)/2, where D.F. is the appropriate distribution factor, and recording the results in the middle column. For example, the carryover to the mid-span of AB from A = [(1 + 0.5/3)/2] x 69 = 40 and from B = -[(1+ 0.5/4)/2] x (-145) = 82. These correction moments are then added to the fixed-end mid-span moment to give the maximum mid-span sagging moment, that is, 733 + 40 + 82 = 855.7.2.3 Column ForcesThe gravity load axial force in a column is estimated from the accumulated tributary dead and live floor loading above that level, with reductions in live loading as permitted by the local Code of Practice. The gravity load maximum column moment is estimated by taking the maximum difference of the end moments in the connected girders and allocating it equally between the column ends just above and below the joint. To this should be added any unbalanced moment due to eccentricity of the girderconnections from the centroid of the column, also allocated equally between the column ends above and below the joint.第七章框架结构高层框架结构一般由平行或正交布置的梁柱结构组成,梁柱结构是由带有能承担弯矩作用节点的梁、柱组成。

土木工程外文文献翻译(含中英文)

土木工程外文文献翻译(含中英文)

Experimental research on seismic behavior of abnormal jointin reinforced concrete frameAbstract :Based on nine plane abnormal joint s , one space abnormal joint experiment and a p seudo dynamic test of a powerplant model , the work mechanism and the hysteretic characteristic of abnormal joint are put to analysis in this paper. A conception of minor core determined by the small beam and small column , and a conclusion that the shear capacity of ab2normal joint depends on minor core are put forward in this paper. This paper also analyzes the effect s of axial compres2 sion , horizontal stirrup s and section variation of beam and column on the shear behavior of abnormal joint . Finally , the formula of shear capacity for abnormal joint in reinforced concrete f rame is provided.Key words : abnormal j oint ; minor core ; seismic behavior ; shear ca paci t yCLC number :TU375. 4 ; TU317. 1 Document code :A Article ID :100627930 (2006) 022*******1 Int roductionFor reinforced concrete f rame st ructure , t he joint is a key component . It is subjected to axialcomp ression , bending moment and shear force. The key is whet her the joint has enough shear capaci2ty. The Chinese Code f or S eismic Desi gn of B ui l di ngs ( GB5001122001) adopt s the following formulato calculate t he shear capacity of the reinforced concrete f rame joint .V j = 1. 1ηj f t b j h j + 0. 05ηj Nb jb c+ f yv A svjh b0 - a′ss(1)Where V j = design value of t he seismic shear capacity of the joint core section ;ηj = influential coefficient of t he orthogonal beam to the column ;f t = design value of concrete tensile st rength ;b j = effective widt h of the joint core section ;h j = dept h of the joint core section , Which can be adopted as t he depth of the column section int he verification direction ;N = design value of axial compression at t he bot tom of upper column wit h considering the combi2 nation of the eart hquake action , When N > 015 f c b c h c , let N = 0. 5 f c b c h c ;b c = widt h of t he column section ;f yv = design value of t he stirrup tensile st rengt h ;A svj = total stirrup area in a set making up one layer ;h b0 = effective dept h of t he beam.If t he dept h of two beams at the side of t he joint is unequal , h b0 = t he average depth of two beams.a′s = distance f rom the cent roid of the compression beam steel bar to the ext reme concrete fiber . s = distance of t he stirrup .Eq. 1 is based on t he formula in t he previous seismiccode[1 ] and some modifications made eavlicr and it is suit2able to the normal joint of reinforced concrete f rame , butnot to t he abnormal one which has large different in t hesection of t he upper column and lower one (3 600 mm and1 200 mm) , lef t beam and right beam (1 800 mm and 1200 mm) . The shear capacity of abnormal joint s calculat2ed by Eq. 1 may cause some unsafe result s. A type of ab2normal joint which of ten exist s in t he power plant st ruc2t ure is discussed ( see Fig. 1) , and it s behavior was st ud2ied based on t he experiment in t his paper2 Experimental workAccording to the above problem , and t he experiment of plane abnormal joint s and space abnormal joint , a p seudo dynamic test of space model of power plant st ruct ure was carried out . The aim of t hisst udy is to set up a shear force formula and to discuss seismic behavior s of t he joint s.According to the characteristic of t he power plant st ruct ure , nine abnormal joint s and one space abnormal joint were designed in t he experiment . The scale of the model s is one2fif t h. Tab. 1 and Tab.2 show t he dimensions and reinforcement detail s of t he specimens.Fig. 2 shows the typical const ruction drawing of t he specimen. Fig. 3 shows the loading set up . These specimens are subjected to low2cyclic loading , the loading process of which is cont rolled by force and displacement , t he preceding yield loading by force and subsequent yield by t he displacement .The shear deformation of the joint core , t he st rain of the longit udinal steel and t he stirrup are main measuring items.3 Analysis of test result s3. 1 Main resultsTab. 3 shows t he main result s of t he experiment .3. 2 Failure process of specimenBased on t he experiment , t he process of t he specimens’failure includes four stages , namely , t he initial cracking , t he t horough cracking , the ultimate stage and t he failure stage.(1) Initial cracking stageWhen t he first diagonal crack appears along t he diagonal direction in t he core af ter loading , it s widt h is about 0. 1mm , which is named initial cracking stage of joint core. Before t he initial cracking stage , t he joint remains elastic performance , and the variety of stiff ness is not very obvious on t hep2Δcurve. At t his stage concrete bear s most of the core shear force while stirrup bears few. At t he timewhen t he initial crack occur s , t he st ress of t he stirrup at t he crack increase sharply and t he st rain is a2bout 200 ×10 - 6 —300 ×10 - 6 . The shear deformation of t he core at t his stage is very small (less than 1×10 - 3 radian ,generally between 0. 4 ×10 - 3 and 0. 8 ×10 - 3 radian) .(2) Thorough cracking stageWit h the load increasing following t he initial cracking stage , the second and t hird crossing diago2 nal cracks will appear at t he core. The core is cut into some small rhombus pieces which will become at least one main inclined crack across t he core diagonal . The widt h of cracks enlarges obviously , andt he wider ones are generally about 0. 5mm , which is named core t horough cracking stage. The st ress of stirrup increases obviously , and the stirrup in t he middle of t he core is near to yielding or has yiel2 ded. The joint core shows nonlinear property on t he p2Δcurve , and it enter s elastic2plastic stage. Theload at t horough cracking stage is about 80 % —90 % load.(3) Ultimate stageAt t his stage , t he widt h of t he cracks is about 1mm or more and some new cracks continue to oc2 cur . The shear deformation at t he core is much larger and concrete begins to collap se. Af ter several cyclic loading , the force reaches the maximum value , which is called ultimate stage. The load increase is due to t he enhancing of the concrete aggregate mechanical f riction between cracks. At t he same timet he st ress of stirrup increases gradually. On t he one hand stirrup resist s t he horizontal shear , and on t he ot her hand the confinement effect to t he expanding compression concrete st rengthens continuous2ly , which can also improve t he shear capacity of diagonal compression bar mechanism.(4) Failure stageAs the load circulated , concrete in t he core began to collap se , and t he deformation increased sharply , while the capacity began to drop . It was found t hat t he slip of reinforcement in t he beam wasvery serious in t he experiment . Wit h t he load and it s circulation time increasing , t he zoon wit houtbond gradually permeated towards t he internal core , enhancing t he burden of t he diagonal compressionbar mechanism and accelerates the compression failure of concrete. Fig. 4 shows t he p hotos of typical damaged joint s.A p seudo dynamic test of space model ofpower plant st ruct ure was carried out to researcht he working behavior of t he abnormal joint s in re2al st ructure and the seismic behavior of st ructure.Fig. 5 shows the p hoto of model .The test includes two step s. The fir st is thep seudo dynamic test . At t his step , El2Cent rowave is inp ut and the peak acceleration variesf rom 50 gal to 1 200 gal . The seismic response is measured. The second is t he p seudo static test . Theloading can’t stop until t he model fail s.Fig. 7 Minor coreThe experiment shows t hat t he dist ribution and development of t hecrack is influenced by t he rest rictive effect of the ort hogonal beam , andt he crack of joint core mainly dist ributes under t he orthogonal beam( see Fig. 6) , which is different f rom t he result of t he plane joint test ,but similar to J 4210.3. 3 Analysis of test results3. 3. 1 Mechanical analysisIn t he experiment , t he location of the initial crack of t he exteriorjoint and the crushed position of concrete both appear in the middle oft he joint core , and t he position is near t he centerline of t he upper col2umn. The initial crack and crushed position of t he concrete of the interior joint both appear in t he mi2 nor core ( see Fig. 4 ,Fig. 7) . For interior abnormal joint t he crack doesn’t appear or develop in t he ma2j or core out side of the mi nor core until t horough cracking takes place , while t he crack seldom appearsin t he shadow region ( see Fig. 7) as the joint fail s. Therefore , for abnormal joint , t he shear capacity oft he joint core depends on t he properties of t he mi nor core , namely , on t he st rengt h grades of concrete ,t he size and the reinforcement of t he mi nor core , get t he effect of t he maj or core dimension can’t be neglected.Mechanical effect s are t he same will that of t he normal joint , when t he forces t ransfer to t he mi2 nor core t hrough column and beam and reinforcement bar . Therefore , t he working mechanisms of nor2mal joint , including t russ mechanism , diagonal compression bar mechanism and rest rictive mechanismof stirrup , are also suitable for mi nor core of t he abnormal joint , but their working characteristic is not symmet rical when the load rever ses. Fig. 8 illust rates t he working mechanism of t he abnormal joint .When t he load t ransfer to mi nor core , t he diagonal compression bar area of mi nor core is biggert han normal joint core2composed by small column and small beam of abnormal joint , which is due to t he compressive st ress diff usion of concrete compressive region of the beam and column , while at t hesame time t he compression carried by the diagonal compression bar becomes large. Because t he main part of bond force of column and beam is added to t he diagonal comp ression bar but cont rasting wit h t he increased area of diagonal compression bar , t he increased action is small . The region in the maj orcore but out of the mi nor core has less st ress dist ribution and fewer cracks. The region can confine t heexpansion of t he concrete of t he mi nor core diagonal compression bar concrete , which enhances t he concrete compressive st rengt h of mi nor core diagonal compression bar .Making t he mi nor core as st udy element , the area increment of concrete diagonal compression barin mi nor core is related to t he st ress diff usion of t he beam and column compressive region. The magni2t ude of diff usion area is related to height difference of t he beam sections and column sections. Name2ly , it is related to t he size of mi nor core section and maj or core section. Thus , the increased shearst rengt h magnit ude caused by mi nor core rest rictive effect on maj or core can be measured quantitative2ly by t he ratio of maj or core area to mi nor core area. And it al so can be expressed that t he rest rictive effect is quantitatively related to t he ratio. Obviously , t he bigger t he ratio is and t he st ronger t he con2finement is , t he st ronger t he bearing capacity is.The region in the maj or core but under the mi nor core still need stirrup bar because of t he hori2 zontal force t ransferred by bigger beam bar . But force is small .3. 3. 2 load2displacement curves analysisFig. 9 shows t he typical load2displacement curves at t he beam end of t he exterior and interiorjoint . The figure showing t hat t he rigidity of t he specimens almo st doesn’t degenerate when t he initialcrack appear s in t he core , and a turning point can be found at t he curve but it isn’t very obvious. Wit ht he crack developing , an obvious t urning point can be found at t he curve , and at t his time , t he speci2men yields. Then t he load can increase f urt her , but it can’t increase too much f rom yielding load to ultimate load. When t he concrete at t he core collap ses and the plastic hinge occured at t he beamend ,t he load begins to decrease rat her t han increase.The ductility coefficient of two kinds of joint s is basically more than 3 (except for J 3 - 9) . But it should be noted t hat the design of specimens is based on the principle of joint core failure. The ratio of reinforcement of beam and column tends to be lower t han practical project s. If t he ratio is larger , t he failure of joint is probably prior to t hat of beam and column , so t he hysteretic curve reflect s t he ductil ity property of joint core.Joint experiment should be a subst ruct ure test (or a test of composite body of beams and col2 umns) . So t he load2displacement curves at t he beam end should be a general reflection of t he joint be2havior work as a subst ruct ure. Providing t hat the joint core fails af ter t he yield of beam and column (especially for beam) , t he load2displacement curves at t he beam end is plump , so the principle of “st rong col umn and weak beam , st ron ger j oi nt" should be ensured which conforms to t he seismic re2sistant principle.The experiment shows t hat t he stiff ness of joint core is large. Before the joint reaches ultimatestage , t he stiff ness of joint core decreases a little and the irrecoverable residual deformation is very small under alternate loading. When joint core enter s failure stage , t he shear deformation increases sharply , and t he stiff ness of joint core decreases obviously , and t he hysteretic curve appears shrink2 age , which is because of t he cohesive slip of beam reinforcement .3. 4 Influential Factors of Abnormal Joint Shear CapacityThe fir st factor is axial compression. Axial compression can enlarge t he compression area of col2 umn , and increase t he concrete compression area of joint core[124 ] . At t he same time , more shearst ransferred f rom beam steel to t he edge of joint core concrete will add to t he diagonal compression bar ,which decreases t he edge shear t hat leads to the crack of joint core concrete. So t he existence of axial comp ression cont ributes to imp roving t he capacity of initial cracks at joint core.The effect of axial compression on t horough cracking load and ultimate load isn’t very obvious[1 ] . The reason is t hat cont rasting wit h no axial compression , the accumulated damage effect of joint coreunder rever sed loading wit h axial compression is larger . Alt hough axial compression can improve t heshear st rengt h of concrete , it increases accumulated damage effect which leads to a decrease of the ad2vantage of axial compression. Therefore t he effect of axial compression on t horough cracking loadandultimate load is not very obvious.Hence , considering the lack of test data of abnormal joint , t he shear capacity formula of abnormal joint adopt 0. 05 nf c b j h j to calculate the effect of axial compression , which is based on the result s of t his experiment and referenced to t he experimental st udy and statistical analysis of Meinheit and J irsa ,et [5 ] .The second factor is horizontal stirrup . Horizontal stirrup has no effect on t he initial crackingshear of abnormal joint , while greatly improves t he t horough cracking shear . Af ter crack appeared , t he stirrup begins to resist t he shear and confines t he expansion of concrete[ 6 ] . This experiment showst hat t he st ress of stirrup s in each layer is not equal . When the joint fail s , t he stirrup s don’t yield simultaneous. Fig. 10 shows t he change of st ress dist ribution of stirrup s along core height wit h t he loadincreasing. Through analyzing test result s , it can be known t hat 80 percent of the height at the joint core can yield.The last factor is the change of sec2tion size of t he beam and column. Thesection change decreases t he initial crack2ing load about 30 p resent of abnormaljoint and makes t he initial crack appear att he position of joint mi nor core. The rea2son for t his p henomenon is t hat small up2per column section makes t he confinementof mi nor core concrete decrease and t heedge shear increase. But t he section change has lit tle effect on thorough cracking load. Af ter t horoughcracking , the joint enter s ultimate state while the external load can’t increase too much , which is dif2 ferent f rom t he behavior of abnormal joint t hat can carry much shear af ter thorough cracking.3. 5 Shear force formula of abnormal jointAs a part of f rame , t he design of joint shall meet t he requirement s of the f rame st ruct ure design , namely , t he joint design should not damage t he basic performance of t he st ruct ure.According to the principle of st ronger j oi nt , it is necessary for joint to have some safety reserva2 tion. The raised cost for conservational estimation of t he joint bearing capacity is small . But t he con2 servational estimation is very important to t he safety of the f rame st ruct ure. At t horough cracking stage , t he widt h of most cracks is more t han 0. 2 mm , which is bigger than t he suggested limit value in t he concrete design code. Big cracks will influence t he durability of st ruct ure. Hence , the bearing capacity at t horough cracking stage is applied to calculating t he bearing capacity of joint . According to t he analysis of t he working mechanisms of abnormal joint , it could be concludedt hat t he bearing capacity of joint core mainly depends on mi nor core when t he force t ransferred f rommaj or core to mi nor core. All kinds of working mechanisms are suitable to mi nor core element . Thus , a formula for calculating t he shear capacity of abnormal joint can be obtained based on Eq. 1. According to the above analysis of influential factor s of shear capacity of abnormal joint , and ref2 erence to Eq. 1 , a formula for calculating t he shear capacity of reinforced concrete f rame abnormal jointis suggested as followsV j = 0. 1ηjξ1 f c b j h j + 0. 1ηj nξ2 f c b j h j +ξ3 f yv A svj h0 - a′s s(2)Where h0 = effective dept h of small beam section in abnormal joint ;ξ1 = influential coefficient consider2ing mi nor core on working as cont rol element for calculating ;ξ2 = influential coefficient considering effect of axial compression ratio , it s value is 0. 5 , andξ3 = influential coefficient considering t hestir2rup doesn’t yield simultaneous , it s value is 0. 8 , n = N/ f c b c h j .From Fig. 8 , the shear capacity of abnormal joint depends on mi nor core , while maj or core has re2st rictive effect on mi nor core. The effect is related to t he ratio of maj or core area to mi nor core area , so assumingξ1 =αA d A x (3)Where A d = area of abnormal joint maj or core , choosing it as t he value of t he dept h of big beam multiplying t he height of lower column ; A x = area of abnormal joint mi nor core , choosing it as t he value oft he depth of small beam multiplying the height of upper column ; andα= parameter to be defined , it s value is 0. 8 derived f rom t he result s of t he experiment ( see Tab. 4)Then Eq. 2 can be replaced byV j = 0. 1ηjαA d A x f c b j h j + 0. 05ηj n f c b j h j + 0. 8 f yv h0 - a′s s(4)4 ConclusionsThe following conclusions can be drawn f rom t his study.(1) The seismic behavior of abnormal joint in reinforced concrete f rame st ruct ure is poor . Af tert horough cracking , t he joint enter s ultimate state while the external load can’t increase too much , andt he safety reservation of joint isn’t sufficient .(2) The characteristic of bearing load of minor core is similar to that of normal joint , but t he area bearing load is different . The shear capacity depend on t he size , t he st rengt h of concrete and the rein2forcement of mi nor core in abnormal joint . The maj or core has rest rictive effect on mi nor core. (3) Joint experiment should be a subst ruct ure test or a test of composite body of beams and col2 umns. Therefore t he load2displacement curves of t he beam end should be a general reflection of t he joint behavior working as a subst ruct ure. Studies of t he hysteretic curve of subst ruct ure should be based on t he whole st ructure. It is critical to guarantee t he stiff ness and st rengt h of joint core in prac2tice.(4) The formula of shear capacity for abnormal joint in reinforced concrete f rame is provided.References[1 ] TAN GJ iu2ru . The seismic behavior of steel reinforced concrete f rame [M] . Nanjing :Dongnan University Press ,1989 :1572163.[2 ] The research group of reinforcement concrete f rame joint . Shear capacity research of reinforced concrete f rame jointon reversed2cyclic loading[J ] . Journal of Building St ructures , 1983 , (6) :9215.[3 ] PAULA Y T ,PARK R. Joint s reinforced concrete f rames designed for earthquake resistance[ R] . New Zealand :De2partment of civil Engineering , University of Canterbury , Christchurch , 1984.[4 ] FU Jian2ping. Seismic behavior research of reinforced concrete f rame joint with the consideration of axialforce[J ] .Journal of Chongqing Univ , 2000 , (5) :23227.[5 ] MEINHEIT D F ,J IRSA J O. Shear st rength of R/ C beam2column connections [J ] . ACI St ructural Journal , 1993 ,(3) :61271.[6 ] KITA YAMA K, OTANI S ,AO YAMA H. Development of design criteria for RC interior beam2column joints ,de2sign of beam2column joint s for seismic resistance[ R] . SP123 ,ACI ,Det roit , 1991 :61272.[7 ] GB5001122001 ,Code for seismic design of buildings [ S] . Beijing : China Architectural and BuildingPress ,2001.钢筋混凝土框架异型节点抗震性能试验研究摘要:基于8个钢筋混凝土框架异型节点的试验研究,分析了异型框架节点的受力与常规框架节点的异同。

土木工程类外文文献翻译---钢筋混凝土可编辑

土木工程类外文文献翻译---钢筋混凝土可编辑

土木工程类外文文献翻译---钢筋混凝土外文文献翻译院系_________________________班级_________________________姓名_________________________指导教师_________________________2012年2月20 日2 外文翻译21 Reinforced ConcretePlain concrete is formed from a hardened mixture of cement water fine aggregate coarse aggregate crushed stone or gravel air and often other admixtures The plastic mix is placed and consolidated in the formwork then cured to facilitate the acceleration of the chemical hydration reaction lf the cementwater mix resulting in hardened concrete The finished product has high compressive strength and low resistance to tension such that its tensile strength is approximately one tenth lf its compressive strength Consequently tensile and shear reinforcement in the tensile regions of sections has to be provided to compensate for the weak tension regions in the reinforced concrete elementIt is this deviation in the composition of a reinforces concrete section from the homogeneity of standard wood or steel sections that requires a modified approach to the basic principles of structural design The two components of the heterogeneous reinforced concrete section are to be so arranged and proportioned that optimal use is made of the materials involved This is possible because concrete can easily be givenany desired shape by placing and compacting the wet mixture of the constituent ingredients are properly proportioned the finished product becomes strong durable and in combination with the reinforcing bars adaptable for use as main members of any structural system The techniques necessary for placing concrete depend on the type of member to be cast that is whether it is a column a bean a wall a slab a foundation a mass columns or an extension of previously placed and hardened concrete For beams columns and walls the forms should be well oiled after cleaning them and the reinforcement should be cleared of rust and other harmful materials In foundations the earth should be compacted and thoroughly moistened to about 6 in in depth to avoid absorption of the moisture present in the wet concrete Concrete should always be placed in horizontal layers which are compacted by means of high frequency power-driven vibrators of either the immersion or external type as the case requires unless it is placed by pumping It must be kept in mind however that over vibration can be harmful since it could cause segregation of the aggregate and bleeding of the concreteHydration of the cement takes place in the presence of moisture at temperatures above 50°F It is necessary to maintain such a condition in order that the chemical hydration reaction can take place If drying is too rapid surface cracking takes place This would result in reduction of concrete strength due to cracking as well as the failure to attain full chemical hydrationIt is clear that a large number of parameters have to be dealt with in proportioning a reinforced concrete element such as geometrical widthdepth area of reinforcement steel strain concrete strain steel stress and so on Consequently trial and adjustment is necessary in the choice of concrete sections with assumptions based on conditions at site availability of the constituent materials particular demands of the owners architectural and headroom requirements the applicable codes and environmental reinforced concrete is often a site-constructed composite in contrast to the standard mill-fabricated beam and column sections in steel structuresA trial section has to be chosen for each critical location in a structural system The trial section has to be analyzed to determine if its nominal resisting strength is adequate to carry the applied factored load Since more than one trial is often necessary to arrive at the required section the first design input step generates into a series of trial-and-adjustment analysesThe trial-and –adjustment procedures for the choice of a concrete section lead to the convergence of analysis and design Hence every design is an analysis once a trial section is chosen The availability of handbooks charts and personal computers and programs supports this approach as a more efficient compact and speedy instructional method compared with the traditional approach of treating the analysis of reinforced concrete separately from pure design22 EarthworkBecause earthmoving methods and costs change more quickly than those in any other branch of civil engineering this is a field where there are real opportunities for the enthusiast In 1935 most of the methods now inuse for carrying and excavating earth with rubber-tyred equipment did not exist Most earth was moved by narrow rail track now relatively rare and the main methods of excavation with face shovel backacter or dragline or grab though they are still widely used are only a few of the many current methods To keep his knowledge of earthmoving equipment up to date an engineer must therefore spend tine studying modern machines Generally the only reliable up-to-date information on excavators loaders and transport is obtainable from the makersEarthworks or earthmoving means cutting into ground where its surface is too high cuts and dumping the earth in other places where the surface is too low fills Toreduce earthwork costs the volume of the fills should be equal to the volume of the cuts and wherever possible the cuts should be placednear to fills of equal volume so as to reduce transport and double handlingof the fill This work of earthwork design falls on the engineer who lays out the road since it is the layout of the earthwork more than anything else which decides its cheapness From the available maps ahd levels the engineering must try to reach as many decisions as possible in the drawing office by drawing cross sections of the earthwork On the site when further information becomes available he can make changes in jis sections and layoutbut the drawing lffice work will not have been lost It will have helped him to reach the best solution in the shortest timeThe cheapest way of moving earth is to take it directly out of the cut and drop it as fill with the same machine This is not always possible but when it canbe done it is ideal being both quick and cheap Draglinesbulldozers and face shovels an do this The largest radius is obtained with the draglineand the largest tonnage of earth is moved by the bulldozer though only over short distancesThe disadvantages of the dragline are that it must dig below itself it cannot dig with force into compacted material it cannot dig on steep slopws and its dumping and digging are not accurate Face shovels are between bulldozers and draglines having a larger radius of action than bulldozers but less than draglines They are anle to dig into a vertical cliff face in a way which would be dangerous tor a bulldozer operator and impossible for a dragline Each piece of equipment should be level of their tracks and for deep digs in compact material a backacter is most useful but its dumping radius is considerably less than that of the same escavator fitted with a face shovelRubber-tyred bowl scrapers are indispensable for fairly level digging where the distance of transport is too much tor a dragline or face shovel They can dig the material deeply but only below themselves to a fairly flat surface carry it hundreds of meters if need be then drop it and level it roughly during the dumping For hard digging it is often found economical to keep a pusher tractor wheeled or tracked on the digging site to push each scraper as it returns to dig As soon as the scraper is fullthe pusher tractor returns to the beginning of the dig to heop to help the nest scraperBowl scrapers are often extremely powerful machinesmany makers build scrapers of 8 cubic meters struck capacity which carry 10 m 3 heaped The largest self-propelled scrapers are of 19 m 3 struck capacity 25 m 3 heaped and they are driven by a tractor engine of 430 horse-powersDumpers are probably the commonest rubber-tyred transport since they can also conveniently be used for carrying concrete or other building materials Dumpers have the earth container over the front axle on large rubber-tyred wheels and the container tips forwards on most types though in articulated dumpers the direction of tip can be widely varied The smallest dumpers have a capacity of about 05 m 3 and the largest standard types are of about 45 m 3 Special types include the self-loading dumper of up to 4 m 3 and the articulated type of about 05 m 3 The distinction between dumpers and dump trucks must be remembered dumpers tip forwards and the driver sits behind the load Dump trucks are heavy strengthened tipping lorries the driver travels in front lf the load and the load is dumped behind him so they are sometimes called rear-dump trucks23 Safety of StructuresThe principal scope of specifications is to provide general principles and computational methods in order to verify safety of structures The safety factor which according to modern trends is independent of the nature and combination of the materials used can usually be defined as the ratio between the conditions This ratio is also proportional to the inverse of the probability risk of failure of the structureFailure has to be considered not only as overall collapse of the structure but also as unserviceability or according to a more precise Common definition As the reaching of a limit state which causes the construction not to accomplish the task it was designed for There are two categories of limit state1 Ultimate limit sate which corresponds to the highest value of the load-bearing capacity Examples include local buckling or global instability of the structure failure of some sections and subsequent transformation of the structure into a mechanism failure by fatigue elastic or plastic deformation or creep that cause a substantial change of the geometry of the structure and sensitivity of the structure to alternating loads to fire and to explosions2 Service limit states which are functions of the use and durability of the structure Examples include excessive deformations and displacements without instability early or excessive cracks large vibrations and corrosionComputational methods used to verify structures with respect to the different safety conditions can be separated into1 Deterministic methods in which the main parameters are considered as nonrandom parameters2 Probabilistic methods in which the main parameters are considered as random parametersAlternatively with respect to the different use of factors of safety computational methods can be separated into1 Allowable stress method in which the stresses computed under imum loads are compared with the strength of the material reduced by given safety factors2 Limit states method in which the structure may be proportioned on the basis of its imum strength This strength as determined by rational analysis shall not be less than that required to support a factored loadequal to the sum of the factored live load and dead load ultimate state The stresses corresponding to working service conditions with unfactored live and dead loads are compared with prescribed values service limit state From the four possible combinations of the first two and second two methods we can obtain some useful computational methods Generally two combinations prevail1 deterministic methods which make use of allowable stresses2 Probabilistic methods which make use of limit statesThe main advantage of probabilistic approaches is that at least in theory it is possible to scientifically take into account all random factors of safety which are then combined to define the safety factor probabilistic approaches depend upon1 Random distribution of strength of materials with respect to the conditions of fabrication and erection scatter of the values of mechanical properties through out the structure2 Uncertainty of the geometry of the cross-section sand of the structure faults and imperfections due to fabrication and erection of the structure3 Uncertainty of the predicted live loads and dead loads acting on the structure4 Uncertainty related to the approximation of the computational method used deviation of the actual stresses from computed stresses Furthermore probabilistic theories mean that the allowable risk can be based on several factors such as1 Importance of the construction and gravity of the damage byits failure2 Number of human lives which can be threatened by this failure3 Possibility andor likelihood of repairing the structure4 Predicted life of the structureAll these factors are related to economic and social considerations such as1 Initial cost of the construction2 Aortization funds for the duration of the construction3 Cost of physical and material damage due to the failure of the construction4 Adverse impact on society5 Moral and psychological viewsThe definition of all these parameters for a given safety factor allows construction at the optimum cost However the difficulty of carrying out a complete probabilistic analysis has to be taken into account For such an analysis the laws of the distribution of the live load and its induced stresses of the scatter of mechanical properties of materials and of the geometry of the cross-sections and the structure have to be known Furthermore it is difficult to interpret the interaction between the law of distribution of strength and that of stresses because both depend upon the nature of the material on the cross-sections and upon the load acting on the structure These practical difficulties can be overcome in two ways The first is to apply different safety factors to the material and to the loads without necessarily adopting the probabilistic criterion The second is an approximate probabilistic method which introduces some simplifyingassumptions semi-probabilistic methods1 中文翻译11钢筋混凝土素混凝土是由水泥水细骨料粗骨料碎石或卵石空气通常还有其他外加剂等经过凝固硬化而成将可塑的混凝土拌合物注入到模板内并将其捣实然后进行养护以加速水泥与水的水化反应最后获得硬化的混凝土其最终制成品具有较高的抗压强度和较低的抗拉强度其抗拉强度约为抗压强度的十分之一因此截面的受拉区必须配置抗拉钢筋和抗剪钢筋以增加钢筋混凝土构件中较弱的受拉区的强度由于钢筋混凝土截面在均质性上与标准的木材或钢的截面存在着差异因此需要对结构设计的基本原理进行修改将钢筋混凝土这种非均质截面的两种组成部分按一定比例适当布置可以最好的利用这两种材料这一要求是可以达到的因混凝土由配料搅拌成湿拌合物经过振捣并凝固硬化可以做成任何一种需要的形状如果拌制混凝土的各种材料配合比恰当则混凝土制成品的强度较高经久耐用配置钢筋后可以作为任何结构体系的主要构件浇筑混凝土所需要的技术取决于即将浇筑的构件类型诸如柱梁墙板基础大体积混凝土水坝或者继续延长已浇筑完毕并且已经凝固的混凝土等对于梁柱墙等构件当模板清理干净后应该在其上涂油钢筋表面的锈及其他有害物质也应该被清除干净浇筑基础前应将坑底土夯实并用水浸湿6英寸以免土壤从新浇的混凝土中吸收水分一般情况下除使用混凝土泵浇筑外混凝土都应在水平方向分层浇筑并使用插入式或表面式高频电动振捣器捣实必须记住过分的振捣将导致骨料离析和混凝土泌浆等现象因而是有害的水泥的水化作用发生在有水分存在而且气温在50°F以上的条件下为了保证水泥的水化作用得以进行必须具备上述条件如果干燥过快则会出现表面裂缝这将有损与混凝土的强度同时也会影响到水泥水化作用的充分进行设计钢筋混凝土构件时显然需要处理大量的参数诸如宽度高度等几何尺寸配筋的面积钢筋的应变和混凝土的应变钢筋的应力等等因此在选择混凝土截面时需要进行试算并作调整根据施工现场条件混凝土原材料的供应情况业主提出的特殊要求对建筑和净空高度的要求所用的设计规范以及建筑物周围环境条件等最后确定截面钢筋混凝土通常是现场浇注的合成材料它与在工厂中制造的标准的钢结构梁柱等不同因此对于上面所提到的一系列因素必须予以考虑对结构体系的各个部位均需选定试算截面并进行验算以确定该截面的名义强度是否足以承受所作用的计算荷载由于经常需要进行多次试算才能求出所需的截面因此设计时第一次采用的数值将导致一系列的试算与调整工作选择混凝土截面时采用试算与调整过程可以使复核与设计结合在一起因此当试算截面选定后每次设计都是对截面进行复核手册图表和微型计算机以及专用程序的使用使这种设计方法更为简捷有效而传统的方法则是把钢筋混凝土的复核与单纯的设计分别进行处理12土方工程由于和土木工程中任何其他工种的施工方法与费用相比较土方挖运的施工方法与费用的变化都要快得多因此对于有事业心的人来说土方工程是一个可以大有作为的领域在1935年目前采用的利用轮胎式机械设备进行土方挖运的方法大多数还没有出现那是大部分土方是采用窄轨铁路运输在这目前来说是很少采用的当时主要的开挖方式是使用正铲反铲拉铲或抓斗等挖土机尽管这些机械目前仍然在广泛应用但是它们只不过是目前所采用的许多方法中的一小部分因此一个工程师为了使自己在土方挖运设备方面的知识跟得上时代的发展他应当花费一些时间去研究现代的机械一般说来有关挖土机装载机和运输机械的唯一可靠而又最新的资料可以从制造厂商处获得土方工程或土方挖运工程指的是把地表面过高处的土壤挖去挖方并把它倾卸到地表面过低的其他地方填方为了降低土方工程费用填方量应该等于挖方量而且挖方地点应该尽可能靠近土方量相等的填方地点以减少运输量和填方的二次搬运土方设计这项工作落到了从事道路设计的工程师的身上因为土方工程的设计比其他任何工作更能决定工程造价是否低廉根据现有的地图和标高道路工程师应在设计绘图室中的工作也并不是徒劳的它将帮助他在最短的时间内获得最好的方案费用最低的运土方法是用同一台机械直接挖方取土并且卸土作为填方这并不是经常可以做到的但是如果能够做到则是很理想的因为这样做既快捷又省钱拉铲挖土机推土机和正铲挖土机都能做到这点拉铲挖土机的工作半径最大推土机所推运的图的数量最多只是运输距离很短拉铲挖土机的缺点是只能挖比它本身低的土不能施加压力挖入压实的土壤内不能在陡坡上挖土而且挖卸都不准确正铲挖土机介于推土机和拉铲挖土机的之间其作用半径大于推土机但小于拉铲挖土机正铲挖土机能挖取竖直陡峭的工作面这种方式对推土机司机来说是危险的而对拉铲挖土机则是不可能的每种机械设备应该进行最适合它的性能的作业正铲挖土机不能挖比其停机平面低很多的土而深挖坚实的土壤时反铲挖土机最适用但其卸料半径比起装有正铲的同一挖土机的卸料半径则要小很多在比较平坦的场地开挖如果用拉铲或正铲挖土机运输距离太远时则装有轮胎式的斗式铲运机就是比不可少的它能在比较平的地面上挖较深的土但只能挖机械本身下面的土需要时可以将土运至几百米远然后卸土并在卸土的过程中把土大致铲平在挖掘硬土时人们发现在开挖场地经常用一辆助推拖拉机轮式或履带式对返回挖土的铲运机进行助推这种施工方法是经济的一旦铲运机装满助推拖拉机就回到开挖的地点去帮助下一台铲运机斗式铲运机通常是功率非常大的机械许多厂家制造的铲运机铲斗容量为8 m3满载时可达10 m3最大的自行式铲运机铲斗容量为19立方米满载时为25 m3由430马力的牵引发动机驱动翻斗机可能是使用最为普遍的轮胎式运输设备因为它们还可以被用来送混凝土或者其他建筑材料翻斗车的车斗位于大橡胶轮胎车轮前轴的上方尽管铰接式翻斗车的卸料方向有很多种但大多数车斗是向前翻转的最小的翻斗车的容量大约为05立方米而最大的标准型翻斗车的容量大约为45m3特殊型式的翻斗车包括容量为4 m3的自装式翻斗车和容量约为05 m3的铰接式翻斗车必须记住翻斗车与自卸卡车之间的区别翻斗车车斗向前倾翻而司机坐在后方卸载因此有时被称为后卸卡车13结构的安全度规范的主要目的是提供一般性的设计原理和计算方法以便验算结构的安全度就目前的趋势而言安全系数与所使用的材料性质及其组织情况无关通常把它定义为发生破坏的条件与结构可预料的最不利的工作条件之比值这个比值还与结构的破坏概率危险率成反比破坏不仅仅指结构的整体破坏而且还指结构不能正常的使用或者用更为确切的话来说把破坏看成是结构已经达到不能继续承担其设计荷载的极限状态通常有两种类型的极限状态即1强度极限状态它相当于结构能够达到的最大承载能力其例子包括结构的局部屈曲和整体不稳定性某此界面失效随后结构转变为机构疲劳破坏引起结构几何形状显著变化的弹性变形或塑性变形或徐变结构对交变荷载火灾和爆炸的敏感性2使用极限状态它对应着结构的使用功能和耐久性器例子包括结构失稳之前的过大变形和位移早期开裂或过大的裂缝较大的振动和腐蚀根据不同的安全度条件可以把结构验算所采用的计算方法分成1确定性的方法在这种方法中把主要参数看作非随机参数2概率方法在这种方法中主要参数被认为是随机参数此外根据安全系数的不同用途可以把结构的计算方法分为1容许应力法在这种方法中把结构承受最大荷载时计算得到的应力与经过按规定的安全系数进行折减后的材料强度作比较2极限状态法在这种方法中结构的工作状态是以其最大强度为依据来衡量的由理论分析确定的这一最大强度应不小于结构承受计算荷载所算得的强度极限状态计算荷载等于分别乘以荷载系数的活载与恒载之和把对应于不乘以荷载系数的活载和恒载的工作使用条件的应力与规定值使用极限状态相比较根据前两种方法和后两种方法的四种可能组合我们可以得到一些实用的计算方法通常采用下面两种计算方法确定性的方法这种方法采用容许应力概率方法这种方法采用极限状态至少在理论上概率法的主要优点是可以科学的考虑所有随机安全系数然后将这些随机安全系数组合成确定的安全系数概率法取决于1制作和安装过程中材料强度的随机分布整个结构的力学性能数值的分散性2截面和结构几何尺寸的不确定性由结构制作和安装造成的误差和缺陷而引起的对作用在结构上的活载和恒载的预测的不确定性所采用的近似计算方法有关的不精确性实际应力与计算应力的偏差此外概率理论意味着可以基于下面几个因素来确定允许的危险率例如建筑物的重要性和建筑物破坏造成的危害性2由于建筑物破坏使生活受到威胁的人数3修复建筑的可能性4建筑物的预期寿命所有这些因素均与经济和社会条件有关例如1建筑物的初始建设费2建筑物使用期限内的折旧费3由于建筑物破坏而造成的物质和材料损失费4在社会上造成的不良影响5精神和心理上的考虑就给定的安全系数而论所有这些参数的确定都是以建筑物的最佳成本为依据的但是应该考虑到进行全概率分析的困难对于这种分析来说应该了解活载及其所引起的盈利的分布规律材料的力学性能的分散性和截面的结构几何尺寸的分散性此外由于强度的分布规律和应力的分布规律之间的相互关系是困难的这些实际困难可以采用两种方法来克服第一种方法对材料和荷载采用不同的安全系数而不需要采用概率准则第二种方法是引入一些而简化假设的近似概率方法半概率方法1建筑工程学院土木工程系土木084班。

土木工程专业英语带译文

土木工程专业英语带译文
如果钢筋等高强度的材料置于混凝土中,则复合材料钢筋混凝土不仅能抵抗 压缩,还能抵抗弯曲和其他直接拉伸作用。 钢筋混凝土部分的混凝土抗压缩和钢 筋抗张力可以制成几乎任何形状和大小的建筑构件。
13
Key characteristics Three physical characteristics give reinforced concrete itsehavior(性能)of reinforced concrete Materials Concrete is a mixture of of Coarse (stone or brick chips) and Fine (generally sand) aggregates with a binder material (usually Portland cement). When mixed with a small amount of water, the cement hydrates form microscopic opaque crystal lattices encapsulating and locking the aggregate into a rigid structure. 混凝土是粗粒(石块或砖块)和细粒(通常是沙粒)与粘结材料(通常是波特兰水泥) 的混合物。 当与少量水混合时,水泥水合物形成微观不透明晶格,将聚集体封装并锁定在 刚性结构中。
Reinforced concrete can be classified as precast or cast in-situ concrete. • 钢筋混凝土可以分为预制或现浇混凝土。
9
• Much of the focus on reinforcing concrete is placed on floor systems. Designing and implementing the most efficient floor system is a key to creating optimal building structures. Small changes in the design of a floor system can have significant impact on material costs, construction schedule, ultimate strength, operating costs, occupancy levels and end use of a building. • 大部分建筑注重加强混凝土的地板系统。 设计和实施最高效的地板系统是 创建最佳建筑结构的关键。 地板系统设计的微小变化会对建筑物的材料成本, 施工进度,最终强度,运营成本,入住率和最终用途产生重大影响。

建筑 土木工程 外文翻译 外文文献 英文文献 混凝土桥梁.doc

建筑 土木工程 外文翻译 外文文献 英文文献 混凝土桥梁.doc

Concrete BridgesConcrete is the most-used construction material for bridges in the United States, and indeed in the world. The application of prestressing to bridges has grown rapidly and steadily, beginning in 1949 with high-strength steel wires in the Walnut Lane Bridge in Philadelphia, Pennsylvania. According to the Federal Highway Administration’s 1994 National Bridge Inventory data, from 1950 to the early 1990s, prestressed concrete bridges have gone from being virtually nonexistent to representing over 50 percent of all bridges built in the United States.Prestressing has also played an important role in extending the span capability of concrete bridges. By the late 1990s, spliced-girder spans reached a record 100 m (330 ft). Construction of segmental concrete bridges began in the United States in 1974.Curretly, close to 200 segmental concrete bridges have been built or are under construction, with spans up to 240 m (800 ft).Late in the 1970s, cable-stayed construction raised the bar for concrete bridges. By 1982, the Sunshine Skyway Bridge in Tampa, Florida, had set a new record for concrete bridges, with a main span of 365 m (1,200 ft). The next year, the Dames Point Bridge in Jacksonville, Florida, extended the record to 400 m (1,300 ft).HIGH-PERFORMANCE CONCRETECompressive StrengthFor many years the design of precast prestressed concrete girders was based on concrete compressive strengths of 34 to 41 MPa (5,000 to 6,000 psi). This strength level served the industry well and provided the basis for establishing the prestressed concrete bridge industry in the United States. In the 1990s the industry began to utilize higher concrete compressive strengths in design, and at the start of the new millennium the industry is poised to accept the use of concrete compressive strengths up to 70 MPa (10,000 psi).For the future, the industry needs to seek ways to effectively utilize even higher concrete compressive strengths. The ready-mixed concrete industry has been producing concretes with compressive strengths in excess of 70 MPa for over 20 years. Several demonstration projects have illustrated that strengths above 70 MPa can be achieved for prestressed concrete girders. Barriers need to be removed to allow the greater use of these materials. At the same time, owners, designers, contractors, and fabricators need to be more receptive to the use of higher-compressive-strength concretes.DurabilityHigh-performance concrete (HPC) can be specified as high compressive strength (e.g., in prestressed girders) or as conventional compressive strength with improveddurability (e.g., in cast-in-place bridge decks and substructures). There is a need to develop a better understanding of all the parameters that affect durability, such as resistance to chemical, electrochemical, and environmental mechanisms that attack the integrity of the material. Significant differences might occur in the long-term durability of adjacent twin structures constructed at the same time using identical materials. This reveals our lack of understanding and control of the parameters that affect durability. NEW MATERIALSConcrete design specifications have in the past focused primarily on the compressive strength. Concrete is slowly moving toward an engineered material whose direct performance can be altered by the designer. Material properties such as permeability, ductility, freeze-thaw resistance, durability, abrasion resistance, reactivity, and strength will be specified. The HPC initiative has gone a long way in promoting these specifications, but much more can be done. Additives, such a fibers or chemicals, can significantly alter the basic properties of concrete. Other new materials, such as fiber-reinforced polymer composites, nonmetallic reinforcement (glass fiber-reinforced and carbon fiber-reinforced plastic, etc.), new metallic reinforcements, or high-strength steel reinforcement can also be used to enhance the performance of what is considered to be a traditional material. Higher-strength reinforcement could be particularly useful when coupled with high-strength concrete. As our natural resources diminish, alternative aggregate sources (e.g., recycled aggregate) and further replacement of cementitious materials with recycled products are being examined. Highly reactive cements and reactive aggregates will be concerns of the past as new materials with long-term durability become commonplace.New materials will also find increasing demand in repair and retrofitting. As the bridge inventory continues to get older, increasing the usable life of structures will become critical. Some innovative materials, although not economical for complete bridges, will find their niche in retrofit and repair.OPTIMIZED SECTIONSIn early applications of prestressed concrete to bridges, designers developed their own ideas of the best girder sections. The result is that each contractor used slightly different girder shapes. It was too expensive to design custom girders for each project.As a result, representatives for the Bureau of Public Roads (now FHWA), the American Association of State Highway Officials (AASHO) (now AASHTO), and the Prestressed Concrete Institute (PCI) began work to standardize bridge girder sections. The AASHTO-PCI standard girder sections Types I through IV were developed in the late 1950s and Types V and VI in the early 1960s. There is no doubt that standardization of girders has simplified design, has led to wider utilization of prestressed concrete for bridges, and, more importantly, has led to reduction in cost.With advancements in the technology of prestressed concrete design and construction, numerous states started to refine their designs and to develop their own standard sections. As a result, in the late 1970s, FHWA sponsored a study to evaluate existing standard girder sections and determine the most efficient girders. This study concluded that bulb-tees were the most efficient sections. These sections could lead toreduction in girder weights of up to 35 percent compared with the AASHTO Type VI and cost savings up to 17 percent compared with the AASHTO-PCI girders, for equal span capability. On the basis of the FHWA study, PCI developed the PCI bulb-tee standard, which was endorsed by bridge engineers at the 1987 AASHTO annual meeting. Subsequently, the PCI bulb-tee cross section was adopted in several states. In addition, similar cross sections were developed and adopted in Florida, Nebraska, and the New England states. These cross sections are also cost-effective with high-strength concretes for span lengths up to about 60 m (200 ft).SPLICED GIRDERSSpliced concrete I-girder bridges are cost-effective for a span range of 35 to 90 m (120 to 300 ft). Other shapes besides I-girders include U, T, and rectangular girders, although the dominant shape in applications to date has been the I-girder, primarily because of its relatively low cost. A feature of spliced bridges is the flexibility they provide in selection of span length, number and locations of piers, segment lengths, and splice locations. Spliced girders have the ability to adapt to curved superstructure alignments by utilizing short segment lengths and accommodating the change in direction in the cast-in-place joints. Continuity in spliced girder bridges can be achieved through full-length posttensioning, conventional reinforcement in the deck, high-strength threaded bar splicing, or pretensioned strand splicing, although the great majority of applications utilize full-length posttensioning. The availability of concrete compressive strengths higher than the traditional 34 MPa (5,000 psi) significantly improves the economy of spliced girder designs, in which high flexural and shear stresses are concentrated near the piers. Development of standardized haunched girder pier segments is needed for efficiency in negative-moment zones. Currently, the segment shapes vary from a gradually thickening bottom flange to a curved haunch with constant-sized bottom flange and variable web depth.SEGMENTAL BRIDGESSegmental concrete bridges have become an established type of construction for highway and transit projects on constrained sites. Typical applications include transit systems over existing urban streets and highways, reconstruction of existing interchanges and bridges under traffic, or projects that cross environmentally sensitive sites. In addition, segmental construction has been proved to be appropriate for large-scale, repetitive bridges such as long waterway crossings or urban freeway viaducts or where the aesthetics of the project are particularly important.Current developments suggest that segmental construction will be used on a larger number of projects in the future. Standard cross sections have been developed to allow for wider application of this construction method to smaller-scale projects. Surveys of existing segmental bridges have demonstrated the durability of this structure type and suggest that additional increases in design life are possible with the use of HPC. Segmental bridges with concrete strengths of 55 MPa (8,000 psi) or more have been constructed over the past 5 years. Erection with overhead equipment has extended applications to more congested urban areas. Use of prestressed composite steel and concrete in bridges reduces the dead weight of the superstructure and offers increased span lengths.LOAD RATING OF EXISTING BRIDGESExisting bridges are currently evaluated by maintaining agencies using working stress, load factor, or load testing methods. Each method gives different results, for several reasons. In order to get national consistency, FHWA requests that all states report bridge ratings using the load factor method. However, the new AASHTO Load and Resistance Factor Design (LRFD) bridge design specifications are different from load factor method. A discrepancy exists, therefore, between bridge design and bridge rating.A draft of a manual on condition evaluation of bridges, currently under development for AASHTO, has specifications for load and resistance factor rating of bridges. These specifications represent a significant change from existing ones. States will be asked to compare current load ratings with the LRFD load ratings using a sampling of bridges over the next year, and adjustments will be proposed. The revised specifications and corresponding evaluation guidelines should complete the LRFD cycle of design, construction, and evaluation for the nation's bridges.LIFE-CYCLE COST ANALYSISThe goal of design and management of highway bridges is to determine and implement the best possible strategy that ensures an adequate level of reliability at the lowest possible life-cycle cost. Several recent regulatory requirements call for consideration of life-cycle cost analysis for bridge infrastructure investments. Thus far, however, the integration of life-cycle cost analysis with structural reliability analysis has been limited. There is no accepted methodology for developing criteria for life-cycle cost design and analysis of new and existing bridges. Issues such as target reliability level, whole-life performance assessment rules, and optimum inspection-repair-replacement strategies for bridges must be analyzed and resolved from a life-cycle cost perspective. To achieve this design and management goal, state departments of transportation must begin to collect the data needed to determine bridge life-cycle costs in a systematic manner. The data must include inspection, maintenance, repair, and rehabilitation expenditures and the timing of these expenditures. At present, selected state departments of transportation are considering life-cycle cost methodologies and software with the goal of developing a standard method for assessing the cost-effectiveness of concrete bridges. DECKSCast-in-place (CIP) deck slabs are the predominant method of deck construction in the United States. Their main advantage is the ability to provide a smooth riding surface by field-adjustment of the roadway profile during concrete placement. In recent years automation of concrete placement and finishing has made this system cost-effective. However, CIP slabs have disadvantages that include excessive differential shrinkage with the supporting beams and slow construction. Recent innovations in bridge decks have focused on improvement to current practice with CIP decks and development of alternative systems that are cost-competitive, fast to construct, and durable. Focus has been on developing mixes and curing methods that produce performance characteristics such as freeze-thaw resistance, high abrasion resistance, low stiffness, and low shrinkage, rather than high strength. Full-depth precast panels have the advantages of significant reduction of shrinkage effects and increased construction speed and have been used in states with high traffic volumes for deck replacement projects. NCHRP Report 407 onrapid replacement of bridge decks has provided a proposed full-depth panel system with panels pretensioned in the transverse direction and posttensioned in the longitudinal direction.Several states use stay-in-place (SIP) precast prestressed panels combined with CIP topping for new structures as well as for deck replacement. This system is cost-competitive with CIP decks. The SIP panels act as forms for the topping concrete and also as part of the structural depth of the deck. This system can significantly reduce construction time because field forming is only needed for the exterior girder overhangs. The SIP panel system suffers from reflective cracking, which commonly appears over the panel-to-panel joints. A modified SIP precast panel system has recently been developed in NCHRP Project 12-41.SUBSTRUCTURESContinuity has increasingly been used for precast concrete bridges. For bridges with total lengths less than 300 m (1,000 ft), integral bridge abutments and integral diaphragms at piers allow for simplicity in construction and eliminate the need for maintenance-prone expansion joints. Although the majority of bridge substructure components continue to be constructed from reinforced concrete, prestressing has been increasingly used. Prestressed bents allow for longer spans, improving durability and aesthetics and reducing conflicts with streets and utilities in urban areas. Prestressed concrete bents are also being used for structural steel bridges to reduce the overall structure depth and increase vertical clearance under bridges. Precast construction has been increasingly used for concrete bridge substructure components. Segmental hollow box piers and precast pier caps allow for rapid construction and reduced dead loads on the foundations. Precasting also enables the use of more complex forms and textures in substructure components, improving the aesthetics of bridges in urban and rural areas. RETAINING WALLSThe design of earth retaining structures has changed dramatically during the last century. Retaining wall design has evolved from short stone gravity sections to concrete structures integrating new materials such as geosynthetic soil reinforcements and high-strength tie-back soil anchors.The design of retaining structures has evolved into three distinct areas. The first is the traditional gravity design using the mass of the soil and the wall to resist sliding and overturning forces. The second is referred to as mechanically stabilized earth design. This method uses the backfill soil exclusively as the mass to resist the soil forces by engaging the soil using steel or polymeric soil reinforcements. A third design method is the tie-back soil or rock anchor design, which uses discrete high-strength rods or cables that are drilled deep into the soil behind the wall to provide a dead anchorage to resist the soil forces.A major advancement in the evolution of earth retaining structures has been the proliferation of innovative proprietary retaining walls. Many companies have developed modular wall designs that are highly adaptable to many design scenarios. The innovative designs combined with the modular standard sections and panels have led to a significant decrease in the cost for retaining walls. Much research has been done to verify thestructural integrity of these systems, and many states have embraced these technologies. RESEARCHThe primary objectives for concrete bridge research in the 21st century are to develop and test new materials that will enable lighter, longer, more economical, and more durable concrete bridge structures and to transfer this technology into the hands of the bridge designers for application. The HPCs developed toward the end of the 20th century would be enhanced by development of more durable reinforcement. In addition, higher-strength prestressing reinforcement could more effectively utilize the achievable higher concrete strengths. Lower-relaxation steel could benefit anchor zones. Also, posttensioning tendons and cable-stays could be better designed for eventual repair and replacement. As our natural resources diminish, the investigation of the use of recycled materials is as important as the research on new materials.The development of more efficient structural sections to better utilize the performance characteristics of new materials is important. In addition, more research is required in the areas of deck replacement panels, continuity regions of spliced girder sections, and safe,durable, cost-effective retaining wall structures.Research in the areas of design and evaluation will continue into the next millennium.The use of HPC will be facilitated by the removal of the implied strength limitation of 70 MPa (10.0 ksi) and other barriers in the LRFD bridge design specifications. As our nation’s infrastructure continues to age and as the vehicle loads continue to increase, it is important to better evaluate the capacity of existing structures and to develop effective retrofitting techniques. Improved quantification of bridge system reliability is expected through the calibration of system factors to assess the member capacities as a function of the level of redundancy. Data regarding inspection, maintenance, repair, and rehabilitation expenditures and their timing must be systematically collected and evaluated to develop better methods of assessing cost-effectiveness of concrete bridges. Performance-based seismic design methods will require a higher level of computing and better analysis tools.In both new and existing structures, it is important to be able to monitor the “health” of these structures through the development of instrumentation (e.g., fiber optics) to determine the state of stresses and corrosion in the members.CONCLUSIONIntroduced into the United States in 1949, prestressed concrete bridges today represent over 50 percent of all bridges built. This increase has resulted from advancements in design and analysis procedures and the development of new bridge systems and improved materials.The year 2000 sets the stage for even greater advancements. An exciting future lies ahead for concrete bridges!混凝土桥梁在美国甚至在世界桥梁上,混凝土是最常用的建设材料。

土木工程专业外文文献及翻译

土木工程专业外文文献及翻译

英文原文:Building construction concrete crack ofprevention and processingAbstractThe crack problem of concrete is a widespread existence but again difficult in solve of engineering actual problem, this text carried on a study analysis to a little bit familiar crack problem in the concrete engineering, and aim at concrete the circumstance put forward some prevention, processing measure。

Keyword:Concrete crack prevention processing ForewordConcrete's is 1 kind is anticipate by the freestone bone, cement, water and other mixture but formation of the in addition material of quality brittleness not and all material。

Because the concrete construction transform with oneself,control etc。

a series problem, harden model of in the concrete existence numerous tiny hole, spirit cave and tiny crack, is exactly because these beginning start blemish of existence just make the concrete present one some not and all the characteristic of quality。

土木工程文献外文翻译(中英互译版)

土木工程文献外文翻译(中英互译版)

使用加固纤维聚合物增强混凝土梁的延性作者:Nabil F. Grace, George Abel-Sayed, Wael F. Ragheb摘要:一种为加强结构延性的新型单轴柔软加强质地的聚合物(FRP)已在被研究,开发和生产(在结构测试的中心在劳伦斯技术大学)。

这种织物是两种碳纤维和一种玻璃纤维的混合物,而且经过设计它们在受拉屈服时应变值较低,从而体现出伪延性的性能。

通过对八根混凝土梁在弯曲荷载作用下的加固和检测对研制中的织物的效果和延性进行了研究。

用现在常用的单向碳纤维薄片、织物和板进行加固的相似梁也进行了检测,以便同用研制中的织物加固梁进行性能上的比较。

这种织物经过设计具有和加固梁中的钢筋同时屈服的潜力,从而和未加固梁一样,它也能得到屈服台阶。

相对于那些用现在常用的碳纤维加固体系进行加固的梁,这种研制中的织物加固的梁承受更高的屈服荷载,并且有更高的延性指标。

这种研制中的织物对加固机制体现出更大的贡献。

关键词:混凝土,延性,纤维加固,变形介绍外贴粘合纤维增强聚合物(FRP)片和条带近来已经被确定是一种对钢筋混凝土结构进行修复和加固的有效手段。

关于应用外贴粘合FRP板、薄片和织物对混凝土梁进行变形加固的钢筋混凝土梁的性能,一些试验研究调查已经进行过报告。

Saadatmanesh和Ehsani(1991)检测了应用玻璃纤维增强聚合物(GFRP)板进行变形加固的钢筋混凝土梁的性能。

Ritchie等人(1991)检测了应用GFRP,碳纤维增强聚合物(CFRP)和G/CFRP板进行变形加固的钢筋混凝土梁的性能。

Grace等人(1999)和Triantafillou(1992)研究了应用CFRP薄片进行变形加固的钢筋混凝土梁的性能。

Norris,Saadatmanesh和Ehsani(1997)研究了应用单向CFRP薄片和CFRP织物进行加固的混凝土梁的性能。

在所有的这些研究中,加固的梁比未加固的梁承受更高的极限荷载。

土木工程中文文献英文翻译

土木工程中文文献英文翻译

Carbon fiber reinforcement technology as a new type of structural reinforcement technology in the construction engineering, is the use of resin bonded materials to the concrete surface,making concrete and carbon fiber to form a composite whole, and work together.At the same time, the technology has the advantages of convenient construction, high strength, wide application and light weight.Therefore, carbon fiber reinforcement technology in the construction defects reinforcement treatment has been widely used, so as to ensure the building bearing ability and stability, improve the shear resistance and bending capacity of building structural members, improve the quality of the whole construction project, achieve the purpose to the building structure reinforcement, and prolong the service life of the building.One, carbon fiber reinforced structural component technology principle.Carbon fiber reinforced structural component technology is the concrete structure of the external paste fiber reinforced composite sheet, both work together in order to achieve the purpose of strengthening.Because the carbon fiber material has good corrosion resistance, high strength, light weight and elastic modulus higher advantages, compared with ordinary steel , the tensile strength of carbon fiber is about ten times that of it, and elastic modulus higher than it.For reinforced concrete structures,the carbon fiber materials we used can be divided into two kinds: carbon fiber material and matching pared with the construction steel, the tensile strength of carbon fiber is ten times and elastic modulus is quite equal to it, even some of the elastic modulus of carbon fiber in it more than two times, and has a good durability and construction performance, so carbon fiber is a very good reinforcement and repair materials.In addition, for supporting resin, including resin of the substrate, the leveling resin and bonding resin, the resin of the substrate and leveling resin have an important role on carbon fiber bonding quality, and bonding resin can make concrete and carbon fiber forming a complex whole, work together, in order to improve the bearing capacity of building structural members, to achieve the purpose of building structure member strengthening.Two,the basic characteristics of carbon fiber materials.1, carbon fiber sheet.According to the mechanical properties of the material, the elastic modulus of the carbonfiber material is not the same.According to the mechanical properties of carbon fiber sheet, the main is the high modulus, high strength and medium modulus.The high modulus carbon fiber cloth is characterized by its low elongation at break but high elastic modulus.The unit weight of carbon fiber cloth is not comparable with that of steel,Carbon fiber sheet is very thin,but because of the chemical structure of carbon fiber, the fiber can be used for any acid salt and all kinds of chemical medium environment, do not be afraid of corrosion and can resist the low temperature or high temperature thermal expansion and contraction.2, supporting resin bonded materials.In the construction project, the main material used in the reinforced concrete structure repair technology is bottom coating,putty,bonding resin or impregnated resin,and its functions are different.First of all, for the bottom coating, the concrete surface is more applicable, can speed up the bond, in order to ensure the stability of the interface.Secondly, for the putty, mainly on various parts of the surface are filled, fill up the gap of the entire surface,so that the function of carbon fiber sheet can be fully played.Then, the bonding resin has the function of sticking to the carbon fiber board, and the impregnated resin has the function of sticking to the carbon fiber cloth.The bonding resin and the impregnated resin are used mainly to bond the carbon fiber sheet to each part of the concrete component, which can make the scattered parts form a whole, and the two work together.In addition, the epoxy resin is mainly applied to the highway concrete bridge, the use of carbon fiber sheet reinforcement technology is also more appropriate,when present in a variety of circumstances, with the change of temperature, it has some influence on its curing properties,therefore, to a large extent, the quality of paste is good or bad, which has an important impact on the number of regular traffic disruption time.Three, strengthening construction technology of carbon fiber reinforced materials.Strengthening construction technology of carbon fiber reinforced materials:unloading--basal treatment--base rubber--leveling--paste--protection.1, unloading.For unloading, it is to remove the non tube components, so that it can make the impact on other components reduce effectively.2, basal treatment.(1)If the concrete surface produces the phenomenons of corrosion, hollowing, honeycomb and spalling,you need to cut out of these parts.For a larger area of poor quality, after the cutting operation, the epoxy mortar should be used to repair the work.(2)For the part that produces the crack,it should be treated in a fully closed manner.(3)For the float, oil and other impurities on the concrete surface,we should use concrete grinder, sandpaper to remove.In addition,to ensure the surface of the component is smooth,polish the raised part of the surface,the corner should make Chamfering processing, and be polished into a circular arc.(4)Before the base operation, must keep the concrete surface dry clean, if not in line with the requirements of the construction, we should use the hair dryer to blow it.3, base rubber.(1)The main agent and curing agent should be placed in the container,the proportion of the main agent and the curing agent must be measured accurately according to the standard of construction,then the electric mixer is used to mix it evenly,determine the amount of the dosage according to the actual temperature of the construction site,and control the use of time strictly , usually run out within an hour.(2)Through the use of roller brush brushing the bottom evenly in the concrete surface,and the next process can be carried out only when the glue is solidified.4, leveling.(1)For leveling operation in Construction Engineering,it can make the difference in height has been further reduced,we can use FE glue level the part of the surface of the concrete which is sunken,template joints and other parts.(2)We can also use FE glue to mend the corner to a smooth arc.5, paste.(1)The size and number of layers of carbon fiber cloth shall be determined according to the actual requirements of the construction.(2)To carry out the deployment and mix of FR glue,and apply it evenly to the position where it needs to be pasted.(3)When the carbon fiber cloth is pasted,no bubbles can be created,if there are bubbles,we can use the special roller along the direction of the fiber to carry out repeated rolling, and makethe FR glue fully soaked carbon fiber cloth.Only when the carbon fiber cloth surface dry ,you can carry on the next layer of paste.(4)Apply FR glue evenly on the surface of the last layer of carbon fiber cloth.6, protection.Plastering and fireproof coating should be adopted to Protect the surface of the reinforced carbon fiber cloth.Four, the application of carbon fiber materials in building structure reinforcement.1, the scope of application of carbon fiber reinforced materials.Applicable to various shapes, any part of the structure, brick masonry reinforcement repair.2,Specification for reinforced concrete structures strengthened with carbon fiber sheets.When the concrete is strengthened by carbon fiber sheet, the component and carbon fiber sheet are bonded together seamlessly,at this time, the carbon fiber sheet and concrete integrate into a whole, together to withstand the stress.3,Carbon fiber sheet can be used in the following ways to strengthen the concrete structural member.When the carbon fiber sheet is used for bending and strengthening of the beam and plate member in the tension zone,the direction of the fiber should be consistent with the direction of the reinforcement;When the beams and columns are subjected to shear and reinforcement,it can be closed U paste or side paste,at this time,fiber direction should be perpendicular to the axial direction of the component;The anti seismic reinforcement of buildings can be pasted fully enclosed,at this time, the fiber direction should be perpendicular to the column axial direction;When there is sufficient evidence, the carbon fiber sheet can also be reinforced according to the stress state of the concrete structure;When the carbon fiber sheet is bonded to the concrete structure, we can according to the national standard, use limit state design method based on probability theory,the ultimate bearing capacity and normal carrying capacity of concrete structures are calculated respectively.Meanwhile,on the one hand, reinforced concrete structure should be based on the nationalstandard, determine the corresponding material design index, and then through the detection to sure its actual strength whether can achieve the relevant requirements;On the other hand,the carbon fiber sheet should be based on the elastic stress-strain curve when the component reaches the limit state to determine the corresponding stress;In general,the ultimate tensile strength of carbon fiber sheet should not be less than 95% of the guaranteed rate of the manufacturer as a marker of the tensile strength.When the member is strengthened with carbon fiber sheet,consideration should be given to the effects of strengthening materials on the components and their properties;As before the use of carbon fiber reinforcement, we should try to remove the live load, in order to reduce the impact on other components.The stress of live load bearing should be fully considered if it can not be completely unloaded.In addition,for members subjected to bending, shear reinforcement,the concrete strength of the strengthened member shall not be less than C15.The strength grade of concrete should not be less than C10 in the whole closed type of reinforcement concrete columns.In short,due to the carbon fiber material has the advantages of all kinds of concrete,Carbon fiber reinforcement technology apply in the construction more and more widely,and become the main reinforcement treatment method of the current construction project,it will have broad application prospects.Building is the infrastructure of city construction, and it plays a very important role in the development of urban modernization.Then with the large number of urban population growth,and with the impact of the environment, load, construction and other factors,the carrying capacity of building structure is gradually reduced,It is necessary to take effective reinforce measures to the building structure in order to improve the bearing capacity of the building structure.It is found that the measures of building structure reinforcement mainly include increasing section method, sticking carbon fiber, applying prestressing tendon, sticking steel plate method and so on,but the prestress method can significantly improve the bearing capacity of the structure, improve the stability of the building structure, security.One, Building structure reinforcement technologyIn the use of building structure,we often found that the beam plate structure appear various problems, such as cracks, steel corrosion, torsion spent large and so on.The cracks in the concrete structure of the building is one of the frequently occurring diseases among these,in the process of the long time use of building structure,under the repeated effects of external loading,it is easy to cause the load cracks in the building structure;In addition,in the construction stage,may be due to various reasons, such as unreasonable ratio of concrete mixture, water cement ratio is not reasonable, the construction process of improper placement and so on,these factors can lead to cracks in the beam structure.If the crack width exceeds a certain range, the bearing capacity of the concrete structure will be greatly reduced.Under the action of earthquake, it is very easy to appear the harm of collapse hazard.Steel corrosion,because the building structure is in the outdoor, the structure is subjected to the action of carbon dioxide for a long time, and the carbonation of concrete occurs.If the carbonation depth of concrete exceeds the protective layer of the reinforcing steel bar, the basic protection of the steel bar can be destroyed,resulting in corrosion of steel reinforcement, and reduce the bonding between steel and concrete,the harms it causes to he carrying capacity of the overall structure of the construction can not be ignored.Therefore, it is necessary to reinforce the building structure effectively.(1)prestressed reinforcement technologyThe prestressed reinforcement is arranged on the beam plate of the building structure, and the prestressing force which is applied to the beam plate forms an external prestressing strengtheningforce system to reinforce the beam plate structure.Prestressed reinforcement technology, its reinforcement effect is obvious, and it can greatly improve the bearing capacity of the building structure, can improve the bearing capacity of 30% ~40%, and can reduce the cracks and structural deformation in the structure.In addition,prestressed reinforcement construction has less impact on the construction of the use of space.Generally,we complete prestressed reinforcement construction under the condition of no restriction on the use of buildings.(2)increasing cross section technologyThis method is widely used in the seismic strengthening of the compression building structure, also can be used in the tensile members, mainly used to strengthen the rod which the raw material has consistent performance , such as steel structure reinforcement.After increasing the cross section of the rod, the strength of the component can be greatly enhanced, and the stability of the structure can be improved.At the same time, it can also be strengthened with reinforced concrete wrapped wooden pieces.(3)pasting steel plate technologyIn this method, the steel plate is pasted on the surface of the structure by the construction adhesive, thereby making full use of the bonding force of the steel plate to make the steel plate and the building structure to be effectively bonded together, to form the two force component.In the bonding structure, the steel plate plays the use of the tensile reinforcing steel bar, which greatly increases the bearing capacity of the structure.Problems should be paid attention to in strengthening:First of all,To remove the paint layer on the surface of the concrete structure, expose the surface of concrete structure; and clean the dust on the surface of concrete structures which is to be reinforced;Secondly, when pasting steel plate,we should avoid strengthening if the air outside is under humid conditions , and to ensure that the temperature of the strengthening of the environment is not higher than 60 degrees.(4)anchorage reinforcement methodThis method is mainly used in the bending and compression member of reinforced concrete.The main principle is to drill holes and inject glue in the original structure,to ensure that the steel bars in the borehole are solidified and rooted.It has good anchorage performance and tensile properties for the steel bars which drill hole is shallow.This method is a new structural strengthening method, and the reinforcement process is relatively simple, and it has less influenceon the force of structure.Matters needing attention for anchorage reinforcement method:This method is suitable to be used in the condition of the ambient temperature above 5 ℃, and the performance of the cementing agent is not damaged;When the environment of strengthening is lower than 5 ℃,we can take the appropriate method to increase the temperature, so that the quality of reinforcement can be ensured.Two, Advantages of prestressed reinforcement on architectureBuilding prestress strengthening technology mainly has the following advantages:First, the reinforcement effect is obvious,it can effectively reduce cracks of the beam plate structure , and extend the service life of the building;Second, prestressed reinforcement construction technology does not reduce the use of space, and greatly improve the carrying capacity of building structure.Third, the prestressing reinforcement construction period is short, the labor force is less, the economy is higher;Four,Prestressed reinforcement of the construction has a small increase in weight,and the maintenance is convenient.Three, The strengthening technology of the construction of our countryIn the actual construction project,for the prestressed reinforcement beams and trusses, the steel boots can be used to anchor nodes;For the frame beam, type steel casing hoop or Perforated bolt can be used to anchor node.3.1 transverse prestressed reinforcement technologyIn the building structure, if the distance between the two ends of the reinforced concrete beam is small, then the two ends of the beam can not conduct prestressed tension operation, then you can use the method of transverse prestressing reinforcement construction.This loading method is mainly install prestressed tendons which is reinforced in the lower edge of the main girder of the symmetrical center line,and we need to curved prestressed reinforcement in suitable position at the end of the beam,then anchor effectively in the end of the main beam of the anchor plate with the support of the fulcrum,its "U" - shaped anchor plate is sheathed on the lower flange of the main beam.Meanwhile,the prestressing tendon is divided into several sections in the horizontal section of the prestressing tendon,and the end of the stick can be used as a fulcrum,in the middle of the prestressing tendon, the tightening bolt is used to tighten the symmetry,prestress is producedin the course of the tension of the prestressing tendon.The study found that this method can effectively reduce the positive moment of middle beam, and can not reduce the shear force at the end of the beam.3.2 longitudinal prestressing reinforcement technologyLongitudinal prestressed reinforcement technology is a reinforcement construction method which apply prestressing tendons portrait along the beam plate.Before the longitudinal prestressing reinforcement,we need to arrange the prestressed tendons along the longitudinal beam,and bend the longitudinal prestressing tendon which is in the position of the end of the beam where sets up guide block,then anchor the longitudinal prestressing tendon on the web plate or top plate of the girder,and stretch prestressing tendon so that the shear force of the end of beam can be reduced effectively.It is found that the longitudinal prestressed reinforcement anchoring structure is mainly longitudinal anchorage structure,which is mainly divided into roof bolting and the web anchor.The advantages of longitudinal prestressed reinforcement is cutting through the amount of concrete in bridge deck,that is the tension construction in the deck operation.In the prestressed reinforcement tensioning operation, we need to pay attention to the tension operation of the symmetrical center line, and the tension operation of the same beam should be synchronized to ensure that the prestressed tendons on both sides of the beam have the same stress state.The prestressed tension program is the same as the prestressed concrete beam.3.3 vertical prestressed reinforcement technologyThe vertical prestressed reinforcement technology is a reinforcement construction method which arranges prestressed tendons symmetrically on both sides of the beam and slab.According to the construction experience,most of the vertical prestressing reinforcement technology do side anchorage in the end of the beam,make vertical tension in the middle of the prestressing tendon,and small cross beams are used to fix the prestressing tendon at the bottom of the beam rib.The vertical prestressed reinforcement method not only has the characteristics of small tension and large tension stroke, but also can effectively overcome the excessive loss of the longitudinal stress,compared with other prestressed reinforcement technology, it has obvious strengthening effect, and can effectively reduce the cracks in the existing building structure.In the construction of vertical prestressed tension, it is needed to carry out piece by piece, and the tension operation needs to be symmetrical to the center line, so as to reduce the loss of elastic compressioneffectively.Four, Concluding remarksTo sum up,with the large number of urban population growth, as well as the environment, load, construction and other factors, the bearing capacity of the construction gradually decreased,so it is necessary to take effective measures to strengthen the building structure to improve the bearing capacity of the building structure.The prestressed reinforcement technology not only can effectively strengthen the building beam and plate, improve the bearing characteristics of the overall structure, but also does not change the shape of the building structure,so that it can improve the stability and safety of the building structure.。

土木工程英文外文文献翻译分析预应力混凝土连续梁毕业设计[管理资料]

土木工程英文外文文献翻译分析预应力混凝土连续梁毕业设计[管理资料]

分析预应力混凝土连续梁1 绪论这次会议是专门讨论结构分析的发展,而不是讨论材料强度,但对材料的认识并用适当的技术分析结构的组成,有助于有效地利用预应力混凝土。

预应力混凝土结构的设计通常是留给专家;粗心将会导致错误或花费更多时间用各种方法寻求解决的方案。

有一些根本性的分歧在预应力混凝土和其他材料之间。

在没有作用荷载下结构依然是受力;可行的解决方案是有限的,在超静定结构,缆索外形的改变会引起不同的自应力,所有这些要素都是受到徐变和温度效应的影响。

如何判别这些问题和如何解决他们呢?自从在十九世纪末Hennebique对钢筋混凝土进行了研究(库萨克1984年),它表明了钢筋和混凝土能更有效地结合起来,如果钢先预制然后把混凝土灌进去。

开裂可以减少,如果可以很好的粘结在一起,这将增加刚度和提高耐久性。

早期尝试,所有失败的原因是由于初始预应力很快消失,留下的结构必须具备一定的承受能力;关于这些情况Leonhardt和Abeles已做出了尝试。

这是Freyssinet对三座桥梁的观察结果,它坐落在维希附近的Allier河上,1927年完成。

用的是预应力混凝土( Freyssinet 1956年)。

只有Boutiron这座桥在二战中保留下来(图1 )。

迄今,它一直假定混凝土的杨氏模量仍然是固定的,但他承认说由于变形的存在,这也解释为何在早期的检测预应力已经损失。

Freyssinet (图2 )因为高强度钢筋已予使用,所以发生徐变后仍然残留有一些预应力,而且同时使用了高质量的混凝土,因此这可减少总体的徐变。

关于Freyssinet的早期预应力混凝土研究是被写在其他地方。

Figure1:Boutiron Bridge,Vic h yFigure 2: Eugen Freyssinet大约在同一时间,这个工作也在英格兰的BRE实验室进行着((格兰维尔1930年)和( 1933 ))。

徐变的发现将归功于谁,受到了争论,但Freyssinet对预应力混凝土的研究和成功的应用是大家都公认的。

5 中英文对照 土木工程 外文翻译 英文文献-混凝土应力实验

5 中英文对照 土木工程 外文翻译 英文文献-混凝土应力实验

混凝土应力实验一、实验介绍直径很小的钢纤维用于混凝土结构可以大大的提高混凝土的抗拉承载能力。

在一般情况下混凝土中掺钢纤维的体积比例在0.2%~2.0%之间。

在很小比例下,钢筋混凝土的张拉响应可假设为不硬化的类型,它有加大单个裂缝扩展性质很像无钢筋的素混凝土,钢纤维对混凝土开裂之后性能的改善作用更加明显,可以通过控制裂缝的开展从而较大幅度地提高混凝土的韧性。

然而它对其它性质的改进很小,因此在正常实验方法下如此低得的纤维含量很难难得到钢纤维混凝土轴拉应力——应变曲线的平稳段。

为了找到一个合适易行的方法来研究SFRC轴拉性能人们做了很多工作并且有报告称可通过添加刚性组件方法来获得轴拉全曲线。

在这篇文章中,我们将用不同类型的纤维来做钢筋混凝土的单轴拉伸试验。

钢筋混凝土的抗拉特型首钢纤维的强度和含量影响。

另外,在强力作用下,钢筋混凝土的应力——应变曲线受多种因素的影响。

对纤维混凝土增强机理进行研究,要获得钢纤维混凝土的受拉全过程曲线,采用轴拉方法最为适宜,但是要在试验方法上作一定改进,并且试验机要有足够的刚度,来保证试验过程的稳定。

众所周知,在工程实践过程中,由于施工技术及经济条件的限制,SFRC中纤维体积掺率一般不超过2%,而大部分工程实例中,纤维掺量都在1%左右。

为此,本文设计了轴拉SFRC材料试验,纤维掺量取1%,并采用不同种类的纤维增强形式,进行对比分析。

二、实验内容试验在60吨万能试验机上进行。

在试验装置中添加了四个高强钢杆以增大试件的卸载刚度,并通过在试件两端添加球铰来消除试件的初始偏心率。

通过调节连接试件和横梁的四个高强螺栓来保证试件的轴心受拉。

试件相对两侧面之间的拉应变值之差不得大于其平均值的15%。

当钢纤维掺量很低(为零或0.5%时),在荷载峰值采用低周反复加载曲线的外包络线来获得轴拉应力——应变全曲线.。

2.1材料由四种不同类型的钢纤维用于该试验,这些纤维中三种是带钩的(和)一种是光滑的。

  1. 1、下载文档前请自行甄别文档内容的完整性,平台不提供额外的编辑、内容补充、找答案等附加服务。
  2. 2、"仅部分预览"的文档,不可在线预览部分如存在完整性等问题,可反馈申请退款(可完整预览的文档不适用该条件!)。
  3. 3、如文档侵犯您的权益,请联系客服反馈,我们会尽快为您处理(人工客服工作时间:9:00-18:30)。

混凝土应力实验一、实验介绍直径很小的钢纤维用于混凝土结构可以大大的提高混凝土的抗拉承载能力。

在一般情况下混凝土中掺钢纤维的体积比例在0.2%~2.0%之间。

在很小比例下,钢筋混凝土的张拉响应可假设为不硬化的类型,它有加大单个裂缝扩展性质很像无钢筋的素混凝土,钢纤维对混凝土开裂之后性能的改善作用更加明显,可以通过控制裂缝的开展从而较大幅度地提高混凝土的韧性。

然而它对其它性质的改进很小,因此在正常实验方法下如此低得的纤维含量很难难得到钢纤维混凝土轴拉应力——应变曲线的平稳段。

为了找到一个合适易行的方法来研究SFRC轴拉性能人们做了很多工作并且有报告称可通过添加刚性组件方法来获得轴拉全曲线。

在这篇文章中,我们将用不同类型的纤维来做钢筋混凝土的单轴拉伸试验。

钢筋混凝土的抗拉特型首钢纤维的强度和含量影响。

另外,在强力作用下,钢筋混凝土的应力——应变曲线受多种因素的影响。

对纤维混凝土增强机理进行研究,要获得钢纤维混凝土的受拉全过程曲线,采用轴拉方法最为适宜,但是要在试验方法上作一定改进,并且试验机要有足够的刚度,来保证试验过程的稳定。

众所周知,在工程实践过程中,由于施工技术及经济条件的限制,SFRC中纤维体积掺率一般不超过2%,而大部分工程实例中,纤维掺量都在1%左右。

为此,本文设计了轴拉SFRC材料试验,纤维掺量取1%,并采用不同种类的纤维增强形式,进行对比分析。

二、实验内容试验在60吨万能试验机上进行。

在试验装置中添加了四个高强钢杆以增大试件的卸载刚度,并通过在试件两端添加球铰来消除试件的初始偏心率。

通过调节连接试件和横梁的四个高强螺栓来保证试件的轴心受拉。

试件相对两侧面之间的拉应变值之差不得大于其平均值的15%。

当钢纤维掺量很低(为零或0.5%时),在荷载峰值采用低周反复加载曲线的外包络线来获得轴拉应力——应变全曲线.。

2.1材料由四种不同类型的钢纤维用于该试验,这些纤维中三种是带钩的(和)一种是光滑的。

试验中所采用的三种混凝土配合比用于研究,见于表一。

在基体强度等级为C60和C80钢纤维混凝土中分别加入了大连建科院生产的DK一5型减水剂和瑞士Sika公司生产的液体减水剂。

这些被用来研究钢纤维混凝土的C30,C60,C80混凝土被制成的试件,在标准情况下养护28天。

三种试件的平均强度见于表一。

水泥采用大连小野田水泥厂生产的32.5级和52.5级普通硅酸盐水泥。

细骨料采用细度模数2.6的河砂。

粗骨料采用5~20 石灰岩碎石。

表一2.2、试件用建筑结构胶将轴拉试件粘贴于两端的钢垫板上。

22组共110个试件的具体参数。

2.3、补充经过28天,普通混凝土和钢纤维混凝土分别被用来做抗拉强度试验。

张拉应力——应变曲线由此获得。

对于高强度钢纤维混凝土诸如抗拉能力等拉伸特性也由此得到。

增强类钢纤维混凝土比增韧类钢纤维混凝土的强度平均提高13%;而由基本开裂至裂缝宽度为0.5mm区间(相应的应变约2000με)的断裂能积分则显示:增韧类钢纤维混凝土比增强类钢纤维混凝土的断裂能平均提高20%.由表3还可以看出,大部分SFRC第一峰值对应的极限拉应变值与素混凝土相当,在100με左右,这说明低含率纤维的掺入对提高混凝土的极限拉应变作用不很明显。

而增韧类SFRC第二峰值对应的应变则大大提高,可达1000με,由此可知第二峰值的出现大大提高了材料的韧性。

DRAMIX型纤维因为长度是其它三种纤维长度的2倍,其断裂韧性更好,在试验曲线中可以看出在应变达到后,其荷载强度仍然保持较高水平,直到10000με应变时荷载仍可保持其峰值水平的50%左右。

三、试验结果和分析3.1 劈拉强度和轴拉极限强度不同试件的劈拉强度和轴拉极限强度查表,在混凝土中增加钢纤维的量可以提高它的劈拉强度和轴拉极限强度,两种不同参数的钢纤维钢筋混凝土和普通混凝土(它们的混合比例相同)的比率也可查表。

3.1.1基体强度及纤维类型对轴拉强度的影响从上我们可以看出钢纤维对初裂强度的增强作用受基体强度变化的影响很小。

也就是说在掺人同种钢纤维时,随着基体强度的增加,钢纤维混凝土与同配比素混凝土的初裂强度的比值基本恒定然而,不同情况下的极限抗拉强度是不一样的,当基体强度增加时,对于不同类型的钢纤维,极限抗拉强度的分配量是不同的。

另外它的增加量比劈拉恰强度大F1型钢纤维作为基体的极限抗拉强度很高,这是因为这类型的钢纤维的强度很高(大于1100MPa)试验过程中没有纤维拔断的现象出现而且当基体强度较高时(C80),钢纤维的端部弯钩被完全拉直。

由于黏结强度的提高,基体强度越高,该纤维对高强混凝土轴拉极限强度的增强效果越好。

F2和F3型钢纤维的强度较高,二者均有端部弯钩,并且表面较为粗糙,当基体强度较高时(C80),出现纤维拔断现象,该现象的出现对这两种钢纤维的增强效果产生了消极影响,因此为了最大限度的发挥这两种钢纤维的增强作用,应将其应用于中高强度混凝土中。

F4型纤维为长直型,其与基体问的粘结力较小,因此它的增强效果耍弱于其他二种。

因为其与基体问的粘结力较小因此在试验过程中没有纤维拔断现象出现。

并且随着基体强度升高,由于黏结力的增大,该纤维增强效率有持续提高。

3.1.2钢纤维掺量对轴拉强度的影响试验中重点针对F3型钢纤维研究了纤维掺量的变化对钢纤维高强混凝土轴拉初裂强度和极限强度的影响。

试验中钢纤维体积掺率变化范围为0.5-1.5。

可见随着纤维掺量增大,轴拉初裂强度和极限强度均有提高。

两图中曲线的上升趋势很相似。

也就是说纤维掺量在整个拉伸过程中对钢纤维混凝土内拉应力的影响是积极的和稳定的。

纤维序号F1 0.642F2 0.862F3 0.794F4 0.589钢纤维钢筋混凝土轴拉极限强度可以用下式来计算:(1)式中:fft为钢纤维钢纤维轴拉极限强度轴拉极限强度;ft为同配比素混凝土轴拉极限强度;纤维类型系数有表四给出为钢纤维体积掺率,l/d 为钢纤维长径比。

3.2 轴拉变形性能和韧性3.2.1 初裂拉应变和峰值荷载拉应变对试件四周四个夹式位移计测得的应变值进行平均获得试件的拉应变值。

若试验中试件相对侧面的拉应变差大于平均值的15%,该试件作废。

高强SFRC的初裂拉应变和峰值拉应变要远大于同配比素混凝土(见表5),随着基体强度或者纤维掺量增大,这个差值有所增长,钢纤维对峰值应变的提高作用要比初裂应变更加明显。

3.2.2 拉伸功和轴拉韧性指数拉伸功为位移0-0.5 mm轴拉荷载位移全曲线下面积(图5中阴影面积)。

另外,引入轴拉韧性指数。

其定义为:(2)式中: fft为钢纤维混凝土轴拉极限强度;A为轴拉试件的破坏横截面面积。

两参数均用来评价钢纤维高强混凝土在轴拉过程中的韧性。

轴拉韧性指数为无量纲系数,与轴拉功相比,在评价轴拉韧性时可在一定程度上消除轴拉极限强度的差别所带来的影响。

从上我们可以发现,基体强度和纤维含量两种参数的有规律的改变很相似,因此我们分析的重点应放在韧性指数上。

掺有四种钢纤维及素混凝土试件基体强度与轴拉韧性指数的关系成比例,其中纤维混凝土试件中钢纤维体积掺率均为1.0%。

可见高强SFRC的轴拉韧性要远远优于同配比素混凝土。

钢纤维的抗拉强度的影响是显著的,随着基体强度升高,混凝土脆性明显增加,素混凝土轴拉韧性明显下降。

在掺有F1和F2型钢纤维的试件中也出现了韧性下降现象。

F1型纤维从基体中拔出其实是一个纤维端钩被拉直,纤维端部周围混凝土被挤碎的过程。

当纤维端钩最终被拉直时,轴拉荷载很快下降。

混凝土的强度越高,基体硬度和脆性越大,上述过程历时也更短。

因此当基体强度较高时,轴拉应力——应变曲线下降得更快,轴拉韧性指数也有所下降。

在四种类型纤维种F1型纤维的增韧效果最好,F2型纤维长径比最小,基体强度较高时出现了纤维拔断现象,因此当基体强度增加时韧性指数不断下降。

F3和F4型钢纤维韧性指数均随基体强度升高而增大。

这两种纤维均为剪切型,表面较粗糙。

在钢纤维和基体之间黏结力的各组分中,摩擦力起主导作用。

摩擦力随基体强度的升高而增大,且该黏结类型的拔出破坏是一个持续过程,因此基体强度升高对掺有这两种钢纤维的混凝土韧性起积极作用。

这两种纤维的不同之处是F3型的两端有弯钩。

由于端钩的存在使得在基体强度不太高时(C30和C60),F3型钢纤维的增韧作用优于F4型。

当基体强度很高时(C80),由于纤维拔断现象影响了F3型的增韧效果,F4型钢纤维的增韧效果叉反过来超过了F3型钢纤维。

3.3钢纤维钢筋混凝土单轴拉伸应力——应变曲线典型的钢纤维高强混凝土轴拉应力一应变全曲线(为了便于比较,每组试件选出条典型曲线作为代表),表述了轴拉曲线随基体强度的变化规律;表述了轴拉曲线随钢纤维(F3型)掺量的变化规律。

曲线由弹性阶段、弹塑性阶段和下降段(软化段)组成。

下降段存在拐点。

从上中可以看到,基体强度越高,轴拉应力一应变全曲线下降得越快。

另外,钢纤维掺量的提高可以大大地改善曲线的丰满程度。

钢纤维类型对轴拉应力一应变全曲线的形状也有一定的影响。

Fl型纤维的曲线是几种钢纤维中最丰满的,并且在拉应变为大约10000个微应变时出现了第二峰值。

该现象体现了Fl型纤维良好的增韧效果。

当基体强度较高时,由于纤维拔断的出现使得F2和F3型钢纤维试件的轴拉曲线下降端呈阶梯状。

F4型纤维的曲线较为平滑,形状与素混凝土曲线相似,但是更为饱满。

这是因为长直形钢纤维的拔出过程是相对连续和柔和的.四、研究分析由4种钢纤维混凝土的典型拉伸应力-应变曲线可以看出:在轴拉条件下,1%掺量的钢纤维远远没有达到使混凝土材料实现应变强化的地步,大部分试验曲线都在达到峰值后,出现荷载骤降段。

但是,随着变形的增加,有两条曲线有明显的第二峰值出现,而另外两条则没有,正是根据这种现象,可以将其分为增强和增韧两大类钢纤维混凝土,有第二峰值的为增韧类,无第二峰值的为增强类。

曾经有许多钢纤维混凝土轴拉应力一应变全曲线模型提出大多数为分段函数,以应力峰值点为分界点。

本文中,全曲线的上升段和下降段采用不同的函数表达式。

在公式(3)中4.1上升段的公式上升段的数学模型为:(4)这里:和为与基体和钢纤维特性有关的参数。

边界条件为:1) X=0,Y=0;2) X=0,dy/dx=E0 /Ep;3)X=1,Y=1,dy/dx=0.由边界条件可得公式(5)可以简化为:(5)系数可以通过试验数据回归获得(6)式中:E0为圆点切线模量;EP 为峰值应力点割线模量(第一峰值)。

因此公式(6)可以转换为:(7)4.2下降段公式下降段数学的模型为:(8)式中:和为与基体和钢纤维特性有关的参数。

下降段表达式中系数值选取1.7。

边界条件x=l和y=1自然满足。

系数的取值通过最小二乘法回归获得:(9)可见基体强度和纤维参量对轴拉曲线下降段的下降速率的影响是相反的。