浮钼尾矿综合回收钼、硫试验研究
钼尾矿综合回收硫铁试验研究
s e c o n d s t a g e ma ne g t i c s e p ra a t i o n.f i n a l l y t h e i r o n c o n c e n t r a t e g r a d e r e a c h e d 6 2 . 7 2 % wh i l e t h e i r o n r e c o v e y r Wa s 4 1 . 8 6 %.
药剂用量单位 :s / t
搅拌 、浮选时间单位 :mi n ;下同
3) I <硫酸 2 0 0
3冰 异丁基黄 药 变量
2木 松醇油 3 5
进行筛分分析 ,筛析结果及金属钼的分布率见表 3 。
表3 尾 矿筛 分 结果
硫粗 I 选 ( 浮选浓度 3 0 %)
厂— _
硫粗精矿
i t w a s v a l u a b l e t o r e c y c l e p y r i t e a n d ma g n e t i t e ro f m t h e mo l y b d e n u m t a i l i n g s .Ad o p t i n g H2 S 0 4 a s a c t i v a t o r , i s o b u t y l x a n t h a t e a s c o l l e c t o r , t e r p e n i c o i l a s f r o t h e r , b y o n c e r o u g h i n g , o n c e c l e a n i n g a n d o n c e s c a v e n g i n g, t h e p y r i t e c o n c e n t r a t e g r a d i n g 4 1 . 21 % S wa s o b t a i n e d b y c l o s e d — c i r c u i t t e s t , a t r e c o v e r y o f 8 7 . 6 8 % .T h e n t h e f l o t a t i o n t a i l i n g s we r e t r e a t e d b y f i r s t s t a g e ma g n e t i c s e p a r a t i o n a n d r e g r i n d i n g a n d
钼尾矿综合回收利用试验报告
钼尾矿综合回收利用试验报告钼尾矿是钼矿选矿过程中产生的一种废弃物,通常被视为资源的浪费和环境问题的来源。
为了最大限度地利用钼尾矿资源,我们进行了一项综合利用的试验研究。
试验方案:首先,我们采集了一定量的钼尾矿,并对其进行物理化学分析。
然后,我们选择了三种相对简单的分离和提取方法进行试验。
这三种方法分别为重力浮选、磁选、和氧气化礼物法。
结果分析:在三种方法中,重力浮选法的回收率最高,但该方法提纯度相对较低。
氧气化礼物法的提纯度最高,但其回收率较低。
磁选法的回收率和提纯度均在中等水平,但该方法需要大量能源和耗时。
经过试验,我们决定采取复合工艺,将重力浮选法和氧气化礼物法进行结合。
具体操作如下:1. 长时间搅拌钼尾矿和乙醇使其达到均匀状态。
2. 使用重力浮选法进行初步的物理分离,将钼碎矿浮在表面,然后进行集中。
分离得到的钼浓缩物中还含有多种杂质,如硫和铁等。
因此,我们需要进一步处理以降低杂质含量。
3. 针对钼浓缩物中的硫和铁等杂质,我们采用氧化礼物法的高温反应处理。
在高温下(超过1000℃),硫和铁将被氧化成SO2和Fe2O3。
在氧气气氛中,SO2会进一步被氧化成SO3,与Fe2O3反应形成具有大量热量的SO2酸渣。
4. 随着高温反应持续进行,锆石、铌和钨等元素中的部分将被氧化并进入SO2酸渣中。
这有助于提高钼的纯度。
5. 通过高速离心,我们可以将SO2酸渣和钼浓缩物分离。
SO2酸渣可以进一步进行处理,以提取其中的其他金属资源。
而钼浓缩物可以进行进一步的提纯和加工。
结论:通过复合工艺,我们成功地实现了钼尾矿的综合回收利用。
我们对提纯率、回收率、能耗以及工艺流程进行了全面考虑。
我们相信,这种综合工艺不仅可以实现资源的最大限度利用,而且还是一种环保、高效的矿产资源综合利用方法。
在试验中,我们对钼尾矿的物理化学特性进行了全面的分析,包括其化学成分、矿物组成以及颗粒分布等。
其中,以下是一些重要的数据:钼尾矿样品:1000克化学成分:Mo:0.08%Fe:34.67%S:11.45%Cu:0.3%Pb:0.01%Zn:0.01%颗粒分布:-200目:39.7%+200目/-325目:40.5%+325目:19.8%矿物组成:黄铁矿:65.2%石英石:11.7%闪锌矿:6.3%褐铁矿:3.6%白云石:3.3%其它:10.9%以上数据表明,钼尾矿主要成分为铁、硫和钼等元素。
钼尾矿综合利用与钼选矿回收率的提高
第3 7卷 第 5期 2 0 1 3年 1 0月
中 国
钼
业
V o 1 . 3 7 No . 5
Oc t o b e r 2 01 3
CHI NA M0LYBDENUM I NDUS TRY
钼 尾 矿 综 合 利 用 与钼 选 矿 回收 率 的提 高
董 盈
1 5 0 0 8 0) ( 黑龙 江省 区域 地质调查所 , 黑龙江 哈尔滨 摘
要: 对多个钼选矿厂 回收率 的考察 中注意到一个共性 的现象 : 选 矿生产 中实现 的钼 回收率 远低 于之前选 矿试
验 的回收率 , 排除 了浮选药剂等工艺 因素 , 基本上都受制 于磨 矿粒 度一 辉钼矿的解离程度 , 进一 步了解发现磨 矿细 度不足 的原 因完全 在于尾矿处置一尾矿在尾矿库 中的沉 降和尾矿 坝 的构 筑。本文依 据几个 钼矿对尾 矿综合 治理
的实践讨论 了无尾清洁选矿对提高 回收率 的作用 , 说 明清 洁生产 不仅对 于环境 , 而且 对于选矿 主工 艺效益 同样 具
有重要 的促进作用 。
关键词 : 尾矿 ; 清洁选 矿 ; 钼 回收率
中 图分 类 号 : T D 9 8 3 文献标识码 : A 文章编号 : 1 0 0 6—2 6 0 2 ( 2 0 1 3 ) 0 5— 0 0 1 5— 0 4
211021691_硫精矿浮选一焙烧综合利用硫酸烧渣中铁试验研究
2023年第3期/第44卷 矿业工程铜精矿铜品位亦有所提高。
3 结 论1)内蒙古某斑岩型铜钼矿产出的混合精矿含铜27.28%、钼2.94%。
矿石中金属矿物主要为黄铜矿及黄铁矿,次为赤铜矿、蓝铜矿、辉钼矿、砷黝铜矿、黝铜矿、辉铜矿、铜蓝、斑铜矿、方铅矿及闪锌矿等。
脉石矿物主要为石英,其次为钾长石、绢云母,其他脉石矿物较少。
混合精矿中黄铜矿及辉钼矿主要呈单体状态存在,少量与硫化矿物连生,极少量呈与脉石矿物连生或被包裹状态。
2)采用新型抑制剂CG4039+NaHS+CG4006组合,在抑制剂总用量为20.80kg/t的条件下,小型闭路试验获得的钼精矿钼品位为53.24%,钼回收率为90.86%。
3)利用MPP进行铜钼分离扩大连续浮选试验,在使用CG4039+NaHS+CG4006组合抑制剂条件下,可获得钼品位48.92%、钼回收率87.92%的钼精矿,铜精矿钼品位为0.41%,铜钼分离效果较好。
4)与现场生产指标相比,新型铜钼分离抑制剂组合可获得更优的分选指标,且药剂没有刺鼻性气味,可改善选矿厂生产环境,实现绿色清洁生产。
[参考文献][1] 杨晓峰,刘瑶瑶.铜钼矿浮选研究现状与进展[J].矿冶,2021,30(6):42-47.[2] 戴新宇,周少珍.我国钼矿石资源特点及其选矿技术进展[J].矿产综合利用,2010(6):28-32.[3] 王怀,郝福来,陆兆锋,等.内蒙古某斑岩型铜钼矿石混合浮选试验研究[J].黄金,2020,41(5):55-59.[4] 赵明福,刘伟,岳辉,等.乌山铜钼矿高次生铜矿石铜钼分离关键技术研究与应用[J].黄金,2014,35(5):55-60.[5] 宋超,赵明福,逄文好,等.斑岩型铜钼矿浮选工艺优化改造与实践[J].黄金,2019,40(10):47-51.[6] 邱丽娜,戴惠新.钼矿的浮选工艺及药剂现状[J].现代矿业,2009,25(7):22-23,38.[7] 符剑刚,钟宏,欧乐明.巯基乙酸在铜钼分离中的应用[J].矿产保护与利用,2002,22(6):38-41.[8] 黄鹏亮,杨丙桥,胡杨甲,等.铜钼分离技术研究进展[J].有色金属(选矿部分),2019(5):50-55,62.ApplicationofanewtypeinhibitortotheflotationofcopperandmolybdenumseparationKangQiuyu牞JinShibin牞ZhengYanping牞PangWenhao牞ZhangHan牞ChenJianlong牞SongChao牗ChangchunGoldResearchInstituteCo.牞Ltd.牘Abstract牶Inthecasestudyofthemixedconcentratesproducedinaporphyrycopper-molybdenumminefromInnerMongolia牞thesmall scaleclosed circuitflotationtestandtheMPPcontinuouspilotflotationtestforcopperandmolybdenumseparationarecarriedoutbyusingthecompositereagentscombiningsulfhydrylnewtypecopperandmolybdenumseparationinhibitorsCG4039牞CG4006牞andNaHS.Theresultsshowwhenthetotaldosageoftheinhibitoris20.80kg/t牞themolybdenumgradeofthemolybdenumconcentrateobtainedbythesmall scaleclosed circuitflota tiontestis53.24%andthemolybdenumrecoveryrateis90.86%牷underthesameconditions牞themolybdenumcon centrateobtainedbytheMPPcontinuouspilotflotationtesthasthemolybdenumgradeof48.92%andmolybdenumrecoveryrateof87.92%.Themolybdenumgradeofthecopperconcentrateis0.41%.Thecopperandmolybdenumseparationoutcomeisgoodandtheindexisbettercomparedtothatonthefield.Keywords牶copperandmolybdenumseparation牷newtypeinhibitor牷porphyrytype牷copper-molybdenumore牷MPPcontinuouspilotflotation矿业工程黄 金GOLD2023年第3期/第44卷硫精矿浮选—焙烧综合利用硫酸烧渣中铁试验研究收稿日期:2022-09-15;修回日期:2023-01-16基金项目:吉林省发改委产业技术研究与开发项目(2020C025-3)作者简介:郎淳慧(1972—),女,高级工程师,从事选矿技术研究工作;E mail:horocyf30@sina.com郎淳慧,张鸣昕,崔商哲,王法春,任洪胜,刘新艳,韩治纬(吉林省冶金研究院)摘要:为综合利用硫酸烧渣中的铁,采用浮选—焙烧工艺对硫酸烧渣原料硫精矿进行提纯除杂试验研究,考察了磨矿细度、抑制剂、捕收剂等对试验指标的影响。
钼尾矿综合利用与钼选矿回收率的提高
钼尾矿综合利用与钼选矿回收率的提高中国钼业钼尾矿综合利用与钼选矿回收率的提高董盈(黑龙江省区域地质调查所,黑龙江哈尔滨150080验的回收率,排除了浮选药剂等工艺因素,基本上都受制于磨矿粒度一辉钼矿的解离程度,进一步了解发现磨矿细度不足的原因完全在于尾矿处置一尾矿在尾矿库中的沉降和尾矿坝的构筑。
本文依据几个钼矿对尾矿综合治理的实践讨论了无尾清洁选矿对提高回收率的作用,说明清洁生产不仅对于环境,而且对于选矿主工艺效益同样具有重要的促进作用。
在考察钼矿选矿回收率的时候,往往注意到或者选择性地忽略掉一个共性的问题,即选矿生产中实际回收率与之前的选矿试验的回收率之间存在较大的差距。
例如河北涞源大湾钼矿分别是78%与85%,河南栾川南泥湖钼矿分别为85%和92%,广东五华白石嶂钼矿74%与85%,差5 ~10个百分点甚至更多。
对于钼这样的重要且稀缺的金属,无论从资源还是效益的角度审视,这个差距都不容小觑,必须找到差距产生的原因并进步探索解决的方法。
1钼选矿回收率损失的分析进步的探究就会发现,造成差距的不在于初选、再磨、扫选等工艺安排,也不在于选矿药剂的抑、-04-08;修改稿返回日期:2013-04-18:董盈(1962―),女,工程师,长期从事地质矿产勘察工改、浮比例,因为这些都可以十分接近于试验条件,只有磨矿粒度指标与试验条件相去甚远,从而成为回收率达不到试验指标的瓶颈。
1.1回收率最大损失是粗、中粒尾砂残留钼南泥湖钼矿的设备、工艺和回收率,在同行业中都属先进,从其几个尾矿样品残留钼的分析可以直观地解释回收率损失的关键。
南泥湖钼尾矿的粒度和钼残留分布见表1.⑴+80目粗粒中残留了7%以上的钼,+140目中、粗粒中残留了原矿总钼的9%以上,约占回收率总损失的2/3;(2)-140目尾矿含钼量小于0.009%,且含钼量与粒径无显著的相关,已不能用辉钼矿解离的彻底与否解释,其中残留的钼应该不能用再磨再选强化解离的办法选出;中国钼业表1南泥湖钼尾矿全粒度分析表目数号样品二号样品平均矿分布钼品位钼分布矿分布钼品位钼分布矿分布钼品位钼分布原矿平均选矿收率(3)如果磨矿细度全部达到-140目,理应能将残留钼全部降低到0.0009%以下(另有测试表明,残留钼0. 001%的临界粒度在100目,但各处矿性不同恐难成为普遍依据),从而挽回5个百分点甚至更多回收率。
从河南栾川浮钼尾矿中综合回收白钨矿的生产实践
关键 词 : 浮铝尾矿; 白钨矿; 浮选; 工艺流程
中图分类 号 :D 8 T 93
文献标识 码 : A
代 残余 结构 , 填 结构 。 充
O 刖 罱
矿石 构造 :主 要为稀 疏浸 染状 构造 ,细 脉状构 造 , 者多 分布 于 夕卡 岩 中, 者 多分 布于 角岩 中 。 前 后
第卷 2 5
解石 等矿物 ,被包裹矿粒 的粒径 一般 小于 0 3 mБайду номын сангаас, . 0m 白钨 矿 中的辉 钼矿 呈均匀 分布 , 以类质 同象形态 存 在 , 含量 变 化 53% ̄ .6% , 均为 29%, 其 _ 03 平 . 用机 械破磨 的方法 很难使 这部分 钨钼解 离 。
矿 物 名称
21 浮选 工艺 .
白矿 钼 母透 透 钨 辉矿云 器
5 5 02 .
绿石萤 泥 石
3 5
综合 回收 白钨 矿是 从辉钼 矿浮选 的尾矿 中直接 回收 , 白钨 粗选采 用 浮选 柱 进行 , 工 艺流程 为: 其 一 次粗 选 , 次扫选 。 一 在此 过程 中用 碳酸钠 调节矿 浆的 D H值 , 白钨 浮选 剂 F 6做 白钨 矿 的捕收剂 。粗 用 X一
金属储 量 6 . 72 5万 t钨 金 属储 量 5 .5万 t , 02 。长 期 以
来, 由于伴生 的 白钨矿 品位 低 、 组分 复 杂 以及 选矿 工 艺、 技术 等 多方面 的原 因, 致使 伴 生 的 白钨矿 没 能得 到及 时回收利用 ,从 而使 具有 较好 经济 价值 的 自钨 资源堆弃在 尾矿库 ,造 成 浪费 。随着 选矿 技术 的进
11 矿石 结构 、 造及 矿石 类型 . 构
() 3 浮钼 尾矿 试样 筛析 结果 如表 3所示 。 () 4 浮钼尾 矿 试样 各矿 物相对 含量 如表 4所 示 。 () 5 白钨矿 的赋 存特 征 。 白钨矿 的化学 组成 为
钼尾矿综合利用研究
钼尾矿综合利用研究范佳志,王伟明(伊春鹿鸣矿业有限公司,黑龙江 伊春 153000)摘 要:在我国,选矿尾矿生产量和堆存量巨大,综合利用率较低。
利用钼尾矿为主要原料,采用烧结法制得微晶玻璃。
此尾矿微晶玻璃的综合性能优于大理石和花岗石,基本达到JC/T872-2000规定的微晶玻璃理化指标。
对钼尾矿的综合开发利用具有一定的指导意义,具有良好的社会效益和经济效益。
关键词:钼尾矿;微晶玻璃;综合利用中图分类号:TD926.4 文献标识码:A 文章编号:1002-5065(2021)02-0141-2Study on Comprehensive Utilization of MolybdenumTailingsFAN Jia-zhi, WANG Wei-ming(Yichun luming Co.,Ltd.,Yichun 153000,China)Abstract: In China, the tailings production and storage are huge, and the comprehensive utilization ratio is low. With molybdenum tailings as the main raw material, glass-ceramics were prepared by sintering method. The comprehensive performance of the tailings glass-ceramics is better than that of marble and granite, and basically reaches the physical and chemical indexes of glass-ceramics stipulated by JC/T872-2000. It has certain guiding significance to the comprehensive development and utilization of tailings, and has good social and economic benefits.Keywords: molybdenum tailings; Microcrystalline glass; Comprehensive using中国是世界上第三大矿业大国,随着经济的快速发展,我国每年的尾矿排放量巨大,若能对这些废弃资源进行综合利用,必然能提高资源的利用率,消除对环境的影响,变废为宝[1-3]。
钼精矿的尾矿处理与终产物综合利用
钼精矿的尾矿处理与终产物综合利用钼精矿是一种重要的金属矿石,广泛应用于钢铁冶炼、合金制备、化工催化剂等领域。
然而,钼精矿的生产和加工过程中产生的大量尾矿却给环境带来了一定的挑战。
尾矿处理和终产物综合利用成为了当前钼精矿行业亟待解决的问题。
尾矿处理是指将钼精矿生产和加工过程中产生的废弃物进行合理处理,以减少环境污染和资源浪费。
对于钼精矿的尾矿处理,主要有以下几种方法:1. 精矿干法浮选法这种方法主要利用颗粒间的差异来实现矿石的分离。
通过在干法浮选设备中利用空气对矿石进行流体化,然后根据矿石中有用矿物和废石的密度差异,采用重力、离心力等原理实现分选。
2. 湿法浮选法湿法浮选法是传统的浮选方法,通过在水中用药剂使矿石和有用矿物发生吸附和离子交换作用,从而使有用矿物浮起,而废石沉淀。
这种方法适用于粒径较细的矿石,可以获得较高的浮选效率。
3. 尾矿重选法尾矿重选是指对已经经过浮选分选的尾矿进行进一步分选,以提高矿石中有用矿物的回收率。
在重选过程中,通过对矿石进行磨碎、遥感识别技术和重力分选等方法,使尾矿中的有用矿物获得更高的浓度。
同时,钼精矿的终产物综合利用也是解决环境问题和资源利用的重要环节。
目前,钼精矿的终产物主要有两种:1. 钼精矿浮选尾渣:这种尾渣主要是浮选过程中未能回收的废渣,它含有一定的钼、砷和硫等有害成分。
对于这种尾渣的综合利用,可以考虑进行资源化利用,如将其作为原料制取钼酸铵等化工产品。
2. 钼精矿冶炼废渣:这种废渣主要是钼精矿在冶炼过程中产生的,含有大量的氧化钼和其他有害物质。
对于这种废渣的综合利用,可以通过矿石焙烧、浸出等技术,提取出其中的有价值金属,如钼、铜等,同时减少对环境的负面影响。
此外,对于钼精矿的综合利用还可以考虑以下措施:1. 辅助矿石的利用:对于大规模的开采,可以采用辅助矿石来替代钼精矿,降低对资源的需求,减少尾矿产生。
2. 循环水利用:合理收集和利用生产过程中产生的废水,经过处理后用于生产和加工过程中的循环使用,减少对水资源的需求。
从栾川浮钼尾矿中综合回收白钨的试验研究
冶联 合 流 程 进 行 了实 验 室 试 验 , 矿 品 位 在 0 1 % 原 .1
的情 况 下 , 得 了精 矿 品 位 为 2 . 3 ~6 . 2 , 获 25% 80 % 回收率 为 4 .2 -8 .6 1 O %- 0 0 %的选 矿 指标 。
其 合理 经 济 效 益 没 能 得 到 实 现 , 栾 川 目前 现 有 按
维普资讯
第 2 6卷 第 4期
20 0 2年 8月
中 国
钼
业
Vo . 6 No 4 12 . Au u t 2 SI Y
从 栾 川 浮钼 尾 矿 中综 合 回 收 白钨 的试 验 研 究
Ke r s M oy d n m , i n s S h ei y wo d lb e u Tal g , c e l e i t
1 前 言
栾 川 钼 矿 田是 世 界 六 大 巨型 钼 矿 田之 一 , 已探
明矿 石储 量 2 1亿 t其 中 钼金 属 量 2 6万 t 居世 界 , 0 , 第 1 ; 生 白钨 6 位 伴 2万 t为 我 国第 二 大 白钨 矿 床 , ,
Z a g Ya h n Xu W e s n hn n o g no g
( u n h a l dn m o L d He a ,7 5 0 L a cu nMo b e u C . t , n n 4 1 0 ) y
Ab ta t Th i a in o c e l ers u c n Lu n h a Sp e e td Te t n C m p e e sv eo e y o sr c est t fsh ei eo rei a c u n Wa rsn e . sso u o t o rh n ie rc v r f sh ei e ea er r n lz . s ut h we t Wa o sbe t e o ey s h eie fo ti n s o c e l ei s v rly a s wee a ay e Re l s o d i S p sil o r c v r c e l r m al g f t n d s t i moy d n m lain i u c u . lb e u f to L a h a o n n n
综合回收中矿中钼、铅、银、硫浮选工艺研究
剂, 铅、 银 的可 泽 陛已受影 响 , 如再采 用 抑铅 浮钼 的优 存特征 : 一种是嵌布于脉石矿物 中的辉钼矿 , 这种辉 先浮选 工艺 可 能会对 贵金 属银 有很 大影 响 , 故 采用 钼 钼 矿 在 脉 石 矿 物 中多 成 辉 钼 矿 “ 阴影 ” , 这 些 辉 钼 矿 铅部分 混合 浮选 一再钼铅分 离工艺 流程 。 从 脉石 中完 全解 离 的难 度 极 大 ;一 种 是完 全鳞 片 状 2 . 2 钼、 铅 混 合浮选 条 件试验 的辉 钼 矿 , 鳞 片 厚度 相 对 比较 大 , 比较 利 于解 离 和 分
钼、 铅 物相 分析 结果 见表 2 。
表 2 试验样钼、 铅 物 相 分 析 结 果 %
物相 分 析结 果 表 明 :试 验 样 中 的 钼矿 物 主 要是 2
选矿工艺研究
辉钼矿 中钼 , 占有率 9 6 . 4 4 %; 铅 矿物 主要是硫化铅 ,
占有率 为 9 3 . 8 2 %。 1 . 3 主要 回收 矿物 赋存 状态 及嵌 布 特征 辉 钼矿 主 要 以鳞 片状 为 主 ,大部 分辉 钼 矿鳞 片 非常薄 , 这 些超 薄 辉 钼矿 在 试验 样 中含量 很 高 , 然而 要 从 赋存 矿 物 中分 离 难度 比较 大 。辉 钼 矿有 三种 赋
精矿
尾矿
图 1磨矿细度试验工艺流程图
蓬
罐
磨矿 细 度 -2 0 0嗣 ( %)
图 2 磨矿细度试验结果
1 . 钼品位 ; 2 . 铅品位 ; 3 . 钼回收率 ; 4 船 回收率
2 . 2 . 2 石 灰 用 量 试 验
因采用 工 艺流 程是 抑 硫 浮钼 铅 的部 分 混合 浮 选 工 艺 流程 , 这 里加 石灰 主 要是 抑制 黄 铁矿 , 试 验 工 艺 流 程见 图 1 , 石 灰 用量试 验 固定 条件 : 煤油 2 0 0 g / t , 丁 黄药 2 0 , 2号油 4 0 。 变 化条 件 : 石 灰用 量分别 为
钼尾矿综合利用与钼选矿回收率的提升
采矿工程M ining engineering 钼尾矿综合利用与钼选矿回收率的提升邹 艳(金堆城钼业集团有限公司,陕西 渭南 714102)摘 要:钼尾矿的开发对于我国经济发展来说是十分重要的,钼尾矿的开发有效的推动了我国经济的发展,同时为我国企业经济的可持续发展做出了突出的贡献。
在钼尾矿中,包含了大量的资源,这些物质资源的价值较高,通过对钼尾矿进行开发可以有效的推动企业的经济发展,为我国的经济建设工作提供助力。
此外,对钼尾矿进行开采也标志着人类的文明在不断的进步,所以说对钼尾矿进行开采具有十分重要的划时代的现实意义。
如果可以实现选矿厂钼尾矿资源的综合利用的话,就很有可能推动新一代资源的改革。
关键词:钼尾矿;可利用资源;综合利用中图分类号:TD926.4 文献标识码:A 文章编号:1002-5065(2020)22-0049-2Comprehensive utilization of molybdenum tailings and improvement of molybdenum recoveryZOU Yan(Jinduicheng Molybdenum Group Co., Ltd,Weinan 714102,China)Abstract: The development of molybdenum tailings is very important for China's economic development. The development of molybdenum tailings effectively promotes the development of China's economy, and makes outstanding contributions to the sustainable development of China's enterprise economy. Molybdenum tailings contain a large number of resources, which are of high value. The development of molybdenum tailings can effectively promote the economic development of enterprises and provide assistance for the economic construction of our country. In addition, the mining of molybdenum tailings also marks the continuous progress of human civilization, so the mining of molybdenum tailings has very important epoch-making practical significance. If the comprehensive utilization of molybdenum tailings resources can be realized, it is likely to promote the reform of a new generation of resources.Keywords: molybdenum tailings; available resources; comprehensive utilization钼尾矿的开发对于人类社会的长久发展来说是十分重要的,对钼尾矿进行开发是实现人类经济文明长久发展和推动社会进步的一个重要标志,是实现可持续性发展社会的一个重要手段。
钼尾矿中有价金属的综合回收研究现状
度较粗,易选; 前景可观;可以 获得 2 种产品; 但缺少精选实验
乙黄药 的钼精矿 ;
研究
S 品位为
27.60%, 回收率为
65.81% 的 硫 精矿
再磨 (-0.037mm 95%),一粗、 七精、三扫
再磨细度要求
煤油、 2# 油、
六偏
Mo 品位 28.22%, 回 收率 64.48%
较高,耗能较大; 流程过长,需 要七次精选
·140·
矿产综合利用
Multipurpose Utilization of Mineral Resources
2021 年
钼尾矿中有价金属的综合回收研究现状
王国彬 ,1,2 蓝卓越 , 1,2,3 赵清平 ,1,3 崔永琦 1, 蔺慧杰 3
(1. 昆明理工大学 国土资源工程学院,云南 昆明 650093; 2. 省部共建复杂有色金属资源清洁利用国家重点实验室,云南 昆明 650093;
广东某 钼矿选 矿老尾矿
88% 左右的钼以硫化钼 形式存在,属易选成分
Mo: 0.0093 SiO2: 77.91 Al2O3:10. 88
一次粗选 一次钼硫分离
粗选
品位为
67.20%, 回收率为
79.49% 的磁
铁矿铁精矿
含钼矿物嵌布粒
煤油、 Mo 品位 2# 油、 为 9%, 硫酸铜、 回收率 硫酸、 为 17.17%
水氧煤玻化油璃钙、、、为为回的457收辉.12.40率钼%9%,
易 选; 可 获 得 2 种产品;两种产 品 中 Mo、Fe 品 位和回收率均较
精矿 高;但流程较长
·142·
矿产综合利用
2021 年
张子瑞 [27]
栾川钼矿 浮选尾矿
钼矿尾矿综合回收试验研究
21 年 1 02 月
中 国 矿 业
CHI A I NG AGAZI N M Nl M NE
Vo1 2 . 1.N o .1
J n 2 1 a. o2
李 琳,吕宪俊,邱 俊,栗 鹏
( 东科技 大学化 学与环境 工程 学 院, 山东 青 岛 2 6 1 ) 山 6 5 O
采 品位 相应 降 低 ,从 而 使 尾 矿 量 激 增 。世 界 各 国 每年排 出的尾矿 量 约 5 0亿 t ,我 国 2 0 0 0年尾 矿 排 放 量 达 6亿 t 右[ 。尾 矿 虽 是 矿 山排 出 的 废 弃 左 1 ]
笔 者针 对 某 钼 矿 选 矿 厂 的尾 矿 进 行 了 选 矿 研 究 , 探 讨 了从 其 中 回 收铁 矿 物 的 可 行 性 ,为 该 厂 尾 矿 的综合利 用提供 了新 的思路 。
LILi n,LU a -u Xinj n,QI J n,LIP n U u eg
( olg fC e sr n n i n na E gn eig h n o gUnv ri f cec n eh oo y,Qig a 6 5 0,C ia C l eo h mitya dE vr me tl n iern ,S a d n iest o i ea d T c n lg e o y S n n d o2 6 1 hn )
分 和铁物 相 组 成 。磁 选 试 验 仪 器 为 实 验 室 磁 选 管 和 鼓形弱 磁选 机 。 2 尾矿 性质分 析
资源综 合 利 用 的 重 要 组 成 部 分 ,也 是 节 约 利 用 矿
产 资 源的一 个 重 要 途 径 。 目前 ,我 国资 源 利 用 率
Ex e i e t lr s a c n s nt e ia e o e y f o a ln so o y d n m i e a s p r m n a e e r h o y h tc lr c v r r m t ii g f m lb e u m n r l
钼精矿的尾矿综合利用与环境风险控制机制
钼精矿的尾矿综合利用与环境风险控制机制钼精矿尾矿是钼矿石经过选矿过程后产生的废弃物,其含有一定量的有害物质,对环境构成潜在的风险。
为了充分利用资源并减少对环境的污染,必须采取综合利用和环境风险控制的措施。
本文将探讨钼精矿尾矿的综合利用方法和环境风险控制机制。
一、钼精矿尾矿的综合利用方法1. 尾矿回收和再利用钼精矿尾矿中含有一定的钼资源,通过合适的技术手段可以回收钼金属,并在其他工业领域再利用。
例如,通过浮选、重选等方法将钼精矿尾矿中的钼金属分离出来,并进行精炼和加工,使其成为具有经济价值的产品。
2. 废矿石堆肥钼精矿尾矿中的矿石经过选矿处理后,依然含有一定量的有用矿物质。
将废矿石进行堆肥处理,可以有效地回收其中的有机物质和营养元素,用于农业土壤改良和植物生长。
这不仅能减少钼精矿尾矿的堆放量,还能实现资源的再利用。
3. 尾矿填埋对于剩余的无法回收和利用的钼精矿尾矿,合理的填埋是一种常见的处理方式。
通过将尾矿填埋在合适的地质环境条件下,有效地隔离和固定其中的有害物质,最大程度减少对环境的影响。
在填埋过程中,需要严格控制渗漏和渗透问题,以及注意填埋场周边环境的监测和保护。
二、环境风险控制机制1. 风险评估与监测在钼精矿尾矿综合利用过程中,需要对环境风险进行全面、系统的评估和监测。
通过评估确定尾矿对水体、土壤和大气等环境介质的潜在风险,并监测其对环境的实际影响。
利用现代化的仪器设备,对周边环境进行定期监测,及时发现和评估环境风险,采取相应的控制措施。
2. 技术改进与创新钼精矿尾矿综合利用的环境风险控制需要依靠技术手段的改进和创新。
在尾矿处理过程中,采用先进的选矿、提取和精炼技术,降低有害物质的含量和释放风险。
借助新型材料和环保设备,改善尾矿处理过程中的资源利用效率和环境保护效果。
3. 监管与政策支持加强对钼精矿尾矿综合利用的监管和政策支持,是确保环境风险控制的重要措施。
相关部门应建立完善的法律法规体系,对尾矿处理企业进行严格的监管和管理。
福建某钼矿选厂尾矿再选试验研究
说 明磨 矿细 度和磨 矿 质量 都 比较差 。 造 。矿床成 因类 型属 中温岩浆热液充填交代型钼矿 多 , ( 2 ) 一 4 0 0 目粒 级 干 筛 与水 筛 的 产 率 相 差 较 大 , 床, 成矿时代为晚侏罗世。 岩矿类型属于斑岩型钼矿 , 未能筛分 矿石 以 细粒 浸 染 型 为 主 。 钼矿 选 厂 尾 矿 Mo品位 为 主要 是 由 于 干 筛过 程 中微 细粒 产 生 团 聚 , 至相 应 粒 级 。 0. 051 %。
( 2 ) 试验 流程 见 图 4 。
3 结 语
( 1 ) 该 钼矿选 厂 尾矿 钼 品位 偏 高 ,主 要是 由于磨 矿 细度 不够 , 造 成钼 矿物 部分 未被 单体 解离 。 ( 2 ) 通 过对 + 1 5 0目粒 级 矿 样 及 其 磨 矿后 矿样 物 相分 析 , 发 现 以下结 果 :  ̄+ 1 5 0 目粒 级 矿样 镜下 检 测结 果 :辉 钼矿 呈 微 细粒 浸染 状嵌 布 于石英 等 脉石 中 。
一
试 验流 程 见 图 2 , 磨 矿 细度 为 一 2 0 0目占 9 9 . 6 2 %。
矿 样
些。
2 . 5 . 2 阶段 磨矿 浮 选试验 ( 1 ) 试 验 流程见 图 3 。
精 矿
尾 矿
图 2 矿样再磨后 浮选流 程
图 3 阶段磨矿浮选试验流程
2 . 3 . 2 浮 选指 标
②在磨矿细度 一 2 0 0目占 9 9 . 6 2 % 时 ,浮选试验 精矿镜下检测结果 : 辉钼矿基本单体解离 。
一
段磨矿 , 达到细度 一 2 0 0目 占 9 9 . 7 1 %, 然 后 再
浮选 。
( 1 ) 试 验流 程 同图 2 。
从河南某钼矿浮选尾矿中综合回收钼和白钨的试验研究
关键 词 : 钨矿; 白 辉钼矿; 水玻璃; 浮选 中图分类 号 : D 5 : D 2 T 94 T 93 文献标 识码 : A
河 南是我 国重要 的钼矿 基地 。钼矿 藏 中伴 生丰 富 的低 品位 白钨 矿 。 由于过 去很 长一段 时 间在 选矿 方面只 单一注重 钼 的回收 , 大量 白钨 当尾 矿丢 弃 。 为
2 试 验 结 果 与分 析
21全 浮脱硫和 钼 浮选试 验 .
合理开 发利用矿 产资源 , 受河 南某 公司 的委托 , 对该
公司 的尾矿 进行 综合 回收钼 和 白钨 的可 选性试 验研 究。 通过试验 确 定 了先浮 辉钼矿 再 浮 白钨矿 的方 案 , 并取得 了较 好 的工艺指 标 。
表 2 7 1氧 化石蜡 皂 用量试验 结果 3
对辉钼矿 的精选 有利 . 但用 量不 宜过 大 . 否则会 对钼
矿物产 生抑制 2 白钨浮选 试验 结果 与分析 . 2
2. . 1白钨浮选捕 收剂 用量 试验 2
白钨粗选 在用 N O 调 浆 到 p 95左 右 , aC , H. 水玻 璃作抑 制剂 , 其用 量 为 40k / 7 1 化石 蜡皂 作捕 . gt 3 氧 , 收剂 的条件下 ,进行 了捕 收剂 7 1 化石 蜡皂 的用 3氧 量试验 。 试验 流程 见 图 3 结果 见表 2 试 验表 明 , , 。 在 7 1 化 石 蜡 皂 的 用 量 为 2 0gt 可 获 得 含 WO 3氧 7 / 时 3 81 、 . % 回收率为 8 . 0 1 2%的 白钨粗 精矿 。 7
试 验 采 用 实 验 室 型 x 20 mx0 MO 4 m 9mm锥 形 球 磨机 , D系 列 的单槽 式 和 挂槽 式浮 选机 ,浮选 XF 试 剂均 使用 工业试 剂 , 中水 玻璃模 数 为 28 其 .。试样 经碎筛 混匀 后装袋 ,单 元试样 质量 3k ,磨矿 细度 g 为一 . 4mm 占 7 0 7 0 0% , 由条 件试 验确定 的。 是
钼尾矿综合利用与钼选矿回收率的提升
钼尾矿综合利用与钼选矿回收率的提升钼尾矿是中国的社会经济和生活不可估量的一笔巨大的财富,不仅可以实现企业经济长期发展,还能实现经济与社会的可持续发展,钼尾矿中含有很多资源,具有很大的价值资源的物质,在对其进行开采是人类文明进步的重要标志,具有划时代的现实意义,实现选矿厂钼尾矿资源的综合利用将会领导新一代资源的改革。
标签:钼尾矿;可利用资源;综合利用钼尾矿的开发是人类社会实现长存发展的必要途径,是促进人类经济文明与社会进步的重要标志,是实现社会可持续发展的基础。
文章主要讲解钼尾矿资源回收的发展,对其资源开发利用的技术创新,结合钼尾矿的开采给社会带来的经济和发展的现实意义,对钼尾矿进行充分的利用。
作为钼矿品位一般都很低,含钼0.1%已属富矿,伴生矿物数量之大、种类之多、涉及之广、技术之杂甚于其他矿种。
钼尾矿的综合回收利用不仅仅指同类矿物如铜矿中的钼、钼矿中的铜、铅、锌、铼等金属矿物或特别稀有贵金属矿物,也应包括金属矿中的非金属矿物或非金属矿中的金属矿物。
1 选矿厂的钼尾矿资源是一种潜在的开发能源(1)在选矿厂中对钼尾矿物质进行加工处理中,对一些没有利用价值的废弃产品进行筛选,钼尾矿里面含有很多可以回收利用的物质,其中可以有效的提高科学技术和现实利用价值,这也就需要我们有效的将其结合起来,等待新技术对其进行开采。
矿业开采技术的发展是一个十分漫长的过程,需要人们不断的去发现它,同时还需要专业技术团队对其进行有效的知识指导,还要长时间的对地理进行勘测才能将它的价值完全的体现出来。
但是现在不少人都只关注后期的价值成分,对矿物前期的价值没有重视,在对矿物进行开采的时候将废弃产品没有重视,对钼尾矿也就没有合理利用,但是近年来由于矿物质的缺乏,对一些可以利用的成分越来越少,科学技术不断的进步,让企业对钼尾矿的处理逐渐重视起来。
(2)钼尾矿是经过漫长过程遗留下来的,人们要对其进行开采加工处理,保证使用的有效性,由于企业对钼尾矿的集中处理,已经分不清钼尾矿由什么物质组成,钼尾矿成了一种复合型很强的特殊矿物质。
钼矿的选矿方法主要是浮选法
====Word行业资料分享--可编辑版本--双击可删====钼矿的选矿方法主要是浮选法,回收的钼矿物是辉钼矿。
有时为了提高钼精矿质量、去除杂质、将钼精矿再进行化学选矿外理。
辉钼矿晶体呈六方层状或板状结构,由沿层间范氏健的S—Mo—S结构和层内极性共价键S—Mo形成的。
层与层间的结合力很弱,而层内的共价键结合力甚强。
所以辉钼矿极易沿结构层间解裂呈片状或板状产出,这是辉铜矿天然可浮性良好的原因。
实践证明:在合适的磨矿细度下,辉钼矿晶体解离发生在S—Mo—S层间,亲水的S—Mo面占很小比例。
但过磨时,S—Mo面的比例增加,可浮性下降,虽然此时加入一定量极性捕收剂如黄药类,有利于辉钼矿的回收,但过磨产生的新矿泥影响浮选效果。
因此对辉钼矿的选别要避免和防止过磨,在生产上需要采用分段磨矿和多段选别流程,逐步达到单体解离,确保钼精矿的高回收率。
钼矿的破碎一般都采用三段一闭路流程,破碎最终产品粒度为12~15毫米。
磨矿通常用球磨机或棒磨-球磨流程。
亨德森是唯一采用半自磨流程的。
浮选采用优先浮选法。
粗选产出钼粗精矿,粗扫选尾矿回收伴生矿物或丢弃。
钼粗精矿采用两、三段再磨,四,五次精选获得最终钼精矿。
钼矿的浮选药剂以非极性油类作捕收剂,同时添加起泡剂。
美国和加拿大用表面活性剂辛太克斯(Syntex)作油类乳化剂。
根据矿石性质,用石灰作调整剂,水玻璃作脉石抑制剂,有时加氰化物或硫化物抑制其他重金属矿物。
为保证钼精矿质量,对钼精矿中所含的铜、铅、铁等重金属矿物和氧化钙以及炭质矿物需进一步进行分离:一般使用硫化钠或硫氢化钠,氰化物或铁氰化物制铜和铁;用重铬酸盐或诺克斯(No kes)抑制铅。
如果使用抑制剂,杂质含量还达不到质量标准,尚需辅以化学选矿处理:次生硫化铜用氰化物浸出;黄铜矿用三氯化铁溶液浸出; 方铅矿用盐酸和三氯化铁溶液浸出,均可达到标准含量。
含氧化钙的脉石易泥化,因此,对于含此类脉石的矿石切忌过磨。
生产上往往添加水玻璃,六聚偏磷酸钠或有机胶作脉石抑制剂或分散剂;也可用活性炭加CMC(羧甲基纤维素)抑制碳酸盐脉石。
- 1、下载文档前请自行甄别文档内容的完整性,平台不提供额外的编辑、内容补充、找答案等附加服务。
- 2、"仅部分预览"的文档,不可在线预览部分如存在完整性等问题,可反馈申请退款(可完整预览的文档不适用该条件!)。
- 3、如文档侵犯您的权益,请联系客服反馈,我们会尽快为您处理(人工客服工作时间:9:00-18:30)。
硫 化 矿物 的活化 作用 要好 于硫 酸 , 合试 验数 据 , 结 确 定 后续 试验 的硫 酸铜 用量 为 9 / 。 0gt
3 2 钼 硫分 离试 验 .
更有 利 于钼矿 物 的 回收 ; 时还 论 证 了该 试 样 更 适 同 合采 用钼 硫混 浮再 分离 的流程 方案 。
摘
要
根 据 试验 矿石 性质 及 系列探 索性试 验 , 有针 对 性 地进 行 了浮 选 药 剂 的种 类 及 用 量研
究 , 果表 明 , 结 该试样 采 用再磨 再 选 工 艺 , 以获 得钼 品位 为 9 0 % 、 含 量 为 1 .6 、 回收 率 可 .0 硫 65% 钼 为 1.7 的钼 精 矿 , 品位 为 2 .0 、 7 1% 硫 76 % 含钼 0 37 、 回收 率 为 6 . 1 、 回收 率 为 1.2 . 1% 硫 58% 钼 4 0 %
注 : u A 含量单位为 g t A 、g /。
1 2 2 浮钼 尾矿 各 矿物相 对 含量 ..
望成为二次资源而被开发利用 ; 同时, 这些尾矿的利
用 也能 显 著减少 对 环境 的危 害 和对耕 地 的 占用 。因
浮 钼尾 矿各 矿物 相对 含量 见 表 2 。
表 2 浮钼尾矿样各 矿物相对 含量 %
花 岗斑岩 型 占全 区金 属 储 量 的 7 ; 晶 正 长 岩 型 % 细
甚少 。
12 浮钼 尾 矿 的性质 .
1 2 1 浮钼 尾矿 化 学成分 分 析结 果 .. 浮 钼尾 矿化 学成 分分 析结 果见 表 1 。
从 表 3可 以 看 出 , 选 厂 浮 钼 尾 矿 中 +0 1 钼 .5 m 粒级 的钼 品位 较 高 , 在 明显 的富集 现象 , m 存 主要 以粗粒 连生 体 为主 , 因此 , 需有 针对 性地 对 尾矿 中的
2 钼 、 原矿性质和 回收前景 硫
该 矿区 中含 钼矿物粒 度较粗 , 易选矿 石 。经 选 属 别 后钼 品位 一般可达 5% 以上 , 0 回收率 在 8% 以上 。 0 浮钼尾矿 的筛析结果及 金属钼 的分布率见 表 3 。
表 3 浮钼 尾 矿 的 筛 析 结 果 及 金 属 钼 的 分布 率
[ ] 中国钨 业 ,04 1 :32 . J. 2 0 ( ) 2 -5
( 收稿 日期 2 1 -83 ) 0 10 -0
61
钼硫 混 浮 硫 酸用 量 试 验采 用 1次 粗选 流 程 , 见 图 1 试 验结 果见 表 5 , 。
表 5 钼 硫 混 浮 粗 选 硫 酸 用 量 试 验 结 果
钼精 矿 , 品位 为 2 .0 、 钼 0 37 、 回收率 硫 76% 含 . 1% 硫 为 6 . 1 、 回收率为 1 .2 的硫精 矿 。在 选 厂 58% 钼 40% 投 资不 大 的情况 下可 以产 生较 为可 观 的经济效 益 。
S ra e ilNo. 0 51 Oc o e . t b r 201 l
现
代
矿
业
总 第 50期 1 21年 l 0 1 O月 第 l 0期
M 0DERN I NG M NI
浮钼 尾 矿 综合 回收钼 、 试 验研 究 硫
张子 瑞 辛 百军 郑 灿辉 刘 亮
( . 钼 集 团钨 业 选矿 一公 司 ;. 钼 集 团矿 山公 司 ) 1洛 2洛
Z n
A u
A g
含 量 2 5
4 2 15 4 8 0 0 2 0 0 .3 0 7 6 0 . .1 .8 .2 .2 0 0 7 .6 .3
也不符合当前国家的节能、 降耗 、 减排政策。随着矿
产 资源 的 大量 开发 利 用 和 原 矿 的 日渐贫 化 , 矿有 尾
P F 2 3F 3 4 i2 2 3 A e O e O SO A1O s
含 量 0 0 5 . 8 0 0 0 2 6 2 0 8 4 . 1 3 9 .5 .6 10 .4 . . 1 .7 8 7 . 0 0 4
成分
C O a O3 【 C F C P a C C Ms o a2 u b
钼 矿 物加 以 回收 。
张子瑞 (9 2 ) 女 , 18 一 , 助理工程师 ,75 0河南省 洛阳市栾 川县 4 10 冷水镇 。
60
张子瑞 辛百 军等 : 浮钼尾 矿综 合 回收钼 试 验研 究 硫 从 该矿 区原 矿分 析 可 知 , 矿石 中还伴 生 有 可 钼
观 的黄 铁 矿 , 品 位 在 1 以 上 , 硫 铁 矿 结 晶 较 硫 % 且 好, 粒度 较粗 , 具有 较好 的可 浮性 。
图 2 钼 硫 分 离 流 程
粗 精 粗尾
表 6 钼 硫 回 收试 验 结 果
图 I 粗 选 条 件 试 验 流 程 表 4 钼 硫 混 浮粗 选 硫 酸铜 用量 试 验 结 果
从表 6可 以看 出 , 精 浓 密脱 药过 程 中加 入 石 混 灰, 浮选分 离 时再加 入 少 量 硫 化钠 对 硫 钼 高 效 分 离
的硫 精 矿 。 关 键词 浮钼尾 矿 钼 硫 混浮 钼硫 分 离
表 1 浮 钼 尾 矿 化 学 成 分 分 析 结果
成分 WO S 3 Mo
在 当前 的选 矿 工 艺 技 术及 设 备 条 件 下 , 矿 中 尾
%
往往 含 有一 定量 的可 综 合 回收利 用 的成 分 , 成 分 该 随着 矿石 性 质 的不 同而不 同。如 栾川 钼矿 钼浮 选尾 矿 中除 了含 少 量 的 钼金 属 外 , 含 有 一 定 量 的钨 、 还 硫 、 、 等 , 接 废 弃 , 仅造 成 矿 产 资 源 的浪 费 , 铁 铜 直 不
收率 为 1.2 的硫 精矿 。 40%
矿 品位 有所 波动 , 钼 硫 回收率 却 呈 现 出 总体 上 升 但
的趋 势 。
3 1 2 硫酸 用量试 验 ..
4 结
论
浮钼 尾 矿 经 过 再 磨 再 选 可 以 获 得 钼 品 位 为
9 O % 、 含量 为 1 . 6 、 回收 率 为 1 . 7 的 .0 硫 65% 钼 7 1%
21年 1 01 0月第 1 0期 从 表 5可 以看 出 , 随着硫酸 铜用 量 的增加 , 精 粗
矿 钼硫 品位 虽有 所提 高 , 钼硫 回收率均 较低 。 但
通 过 以上试 验 结果 的 比较 可 以看 出 , 酸铜 对 硫
3 试 验 研 究 及 结果
试 验首 先 论 证 了不 磨 矿 、 粗粒 级 磨 矿 以及 全 浆 磨矿 , 然后 再 选方 案 论证 , 结果 表 明 , 全浆 磨 选 方 案
交代残余结构及充填结构。
矿石 的构 造 主 要 为稀 疏 浸 染状 构造 , 细脉 状 构 造 , 者 多分 布 于矽 卡 岩 中 , 者 多 分 布 于 角 岩 中 。 前 后
角砾 状构 造仅 在 断层 带 附近产 出。
矿石 的类型主要为矽卡岩型 , 占全区金属储量
的 5% ; 1 长英 角 岩 占全 区金 属储 量 的 3 % ; 为 透 4 次 辉石 角岩 、 长 石 角 岩 型 , 斜 占全 区金 属 储 量 的 8 ; %
十分 有效 , 验 取 得 了 钼 品位 为 9 0 % 、 含 量 为 试 .0 硫
1.6 、 回 收率 为 1 .7 的 钼 精 矿 , 品 位 为 65% 钼 7 1% 硫
2 .0 、 钼 0 3 7 、 回收 率 为 6 . l 、 回 76% 含 . 1% 硫 58% 钼 从 表 4可 以看 出 , 随着硫 酸 铜用量 的增 加 , 精 粗
此, 从浮钼尾矿 中综合 回收钼、 硫既具有显著的经济 意义 , 又具 有重 大 的社会 意 义 。
1 矿 石 性 质
1 1 矿石 结构 、 造及 矿石 类 型 . 构
矿石 的结 构 主要分 为 片状、 状 、 射 状 , 束 放 自 形 一半 自形粒 状 结 构 , 嵌 结 构 , 次 为包 体 结 构 、 镶 其
参 考 文 献
[ ] 张 燕 红 , 文 松 . 栾 川 浮钼 尾 矿 中综 合 回收 白钨 的 试 验 研 究 1 徐 从 [] 中国钼 业 ,02 4 :4 1 . J. 20 ( ) 1 .7 [ ] 周 士 强 , 志 强 , 红 勤. 浮 选 尾 矿 中 回 收 白钨 矿 试 验 研 究 2 石 周 从
钼硫 粗 精
钼硫 混 浮 硫 酸铜 用 量试 验 采 用 1次 粗 选 流程 ,
见 图 1试验 结果 见表 4 , 。
给 矿 : 油8 gt 煤 0/
: Ogt 2油8 『 : 酸铜 、硫 酵 变 量 硫 : 黄药 8 / 乙 0 t g
钼硫 分 离
钼 精 矿
硫 精 矿
3 1 钼硫 混浮 粗选 活化 剂选择 及 用量试 验 .
3 1 1 硫 酸铜 药 剂是 抑 制 剂 , 试验 分 别 进行 了单 一用 石灰 、 单一 用硫 化钠 、 混精 浓密 脱药
后 以石 灰为 主硫 化 钠 为 辅 等 3种 条 件 下 的 分 离 试 验, 3组试 验均 是在 各 自最优 用 量条 件 下 进行 的 , 试 验 流程 见 图 2 试 验 结果见 表 6 , 。