CPHL-37 Slide Hinge Painted Parts Inspection Standard
CPHL-37 滑板铰链喷涂部品检查标准
NO.: Veb.:A/0
Issued date : June.13,2007
发行日期:2007-10-07
Issued: Amphenol Phoenix Hangzhou Telecom parts co.,LTD 发行:杭州安费诺飞凤通信部品有限公司
Contents:
目录
1 Visual Quality (3)
2 Thickness measurement (6)
3.Thermal Shock Test温度冲击测试 (6)
4 Damp heat cyclic Test 交变湿热测试 (8)
5 Solvent Resistance 耐溶剂性能测试 (9)
6 Salt mist endurance 盐雾测试 (9)
7 UV Radiation endurance 抗紫外线老化测试 (10)
8 Adhesion Test 附着力测试 (10)
9 Wearing endurance 耐磨性测试 (11)
10 Hardness Test 硬度测试 (11)
11 Relevant documentation/standard参考文件.................................... (11)
1 Visual Quality 视检
1.1 Visual inspection should be carried out under below condition:
检查应该在下列环境下进行:
1.1.1 Illumination: D65 light source -CIE Standard illuminant ISO10526:1999 (E);
视检应该在D65光源条件下进行;
1.1.2 Viewing time for each part: 10 seconds;
每个部品的检查时间:10秒;
1.1.3 Inspection distance from products: 30cm;
检查产品的距离:30cm;
1.2 Painted surfaces quality according Class I;
对于喷涂区域,检查标准按照Class I标准执行
Other surfaces according Class III;
其它区域检查标准按照Class III标准执行:
Class I :Surfaces which are frequently visible in normal use but require good visual quality .
等级I:对于客户在正常使用下经常看的到的表面且需要较好的外观品质的标准,例如:镜片、手机外壳等。
Class III : Inner Surfaces which are never visible to customer in final product and do not require good visual quality.
等级三: 对于在客户的成品中不可见的内部面、外观品质要求不高的标准。
1.3 The minimum painting area ( see above picture)
喷涂区域(详见下图);
2 Thickness measurement
2.1 The measurement location is as below(Points marked with arrows);
测量位置如下图所示(用箭头标注的点);
2.2 The standard for painting thicknesses of Sheet-1 refer to customer’s otherwised requirement
Sheet-1的喷涂厚度标准参照客户另外的要求;
Location 1
Location 2
Location 3 Location 4
Location 5 Location 6
注:
除要求的喷涂区域需进行喷涂外,其它部位不允许喷涂; Remark:
Do not paint out of the painting area.
Painted Colour: Blue(蓝色)
Thickness requirements:
底漆(16~22um)、面漆(8~12um)、清漆(22~28um);
Painted Colour:Silver(银色)
Thickness requirements:
底漆(18~22um)、面漆(6~10um)、清漆(22~28um);
Painted Colour:Iron-gray(铁灰色)
Thickness requirements:
底漆(18~22um)、面漆(8~12um)、清漆(22~28um);
3.Thermal Shock Test温度冲击测试
a) Low Tem.:-40℃±2℃;high Tem.:85℃±2℃ ,2hour/2hour per each condition,transfer time:15s (lower than 3min) .total cycle: 5cycles(totally 20hours);
-40° / +85°C 各2小时,此为一个循环,共5个循环,(20小时)温度切换时间15s(不大于3分钟);。
b) No visiable decomposition, No mechanical decomposition,Electrical value<1ohm. Adhesion test classification:0-1grade;
不允许有任何外观不良,如变形,白化,变色;
4. UV Radiation endurance 抗紫外线老化测试
a)Test requirement: Put the parts into QUV/Se Accelerate Aging Tester(Amercian), The test
consists of 12 cycles, each cycle being 8 h long, total test period is then 96 hours. One cycle consists of 4 hours UV exposure (UV-A, 340 nm, 60 ︒C, ∆E-value ≤ 0.7) and then 4 hours moisture exposure (50 ︒C).