聚乙烯醇纤维增强水泥基复合材料在长期浸泡作用下抗硫酸盐侵蚀性能_刘曙光(1)
合集下载
相关主题
- 1、下载文档前请自行甄别文档内容的完整性,平台不提供额外的编辑、内容补充、找答案等附加服务。
- 2、"仅部分预览"的文档,不可在线预览部分如存在完整性等问题,可反馈申请退款(可完整预览的文档不适用该条件!)。
- 3、如文档侵犯您的权益,请联系客服反馈,我们会尽快为您处理(人工客服工作时间:9:00-18:30)。
(School of Mines,Inner Mongolia University of Technology,Hohhot 010051,China)
Abstract: In order to research the effect of fiber and fly ash on resistance of polyvinyl alcohol fiber reinforced cementitious composites(PVA fiber/cement composites)to sulfate attack under long-term immersion,the research was done by analyzing morphology change, quality change, volume change, compressive strength and microstructure of the samples tested after several experimental periods.The results of the experiments show that the fiber incorporation with good distribution forming excellent network distribution structure in matrix slows down the erosion rate of PVA fiber/cement composites in sodium sulfate solution,but there is the best content for the fiber incorporation.The fly ash corporation solids PVA fiber/cement composites,and obviously improves resistance of PVA fiber/cement composites to sulfate attack with increasing doping content under mass fraction of 50% . Keywords: polyvinyl alcohol fibers;cementitious composites;sulfate resistance;quality change;volume change; intensity change
项 目 (NJZY12058;13104);内 蒙 古 工 业 大 学 科 学 研 究 项 目 (ZS201137) 通 讯 作 者 :刘 曙 光 ,硕 士 ,教 授 ,博 士 生 导 师 ,主 要 从 事 混 凝 土 基 本 理 论 与 研 究 工 作 E-mail:liusg6011@126.com
刘曙光* ,赵晓明,张 菊,闫长旺
(内蒙古工业大学 矿业学院,呼和浩特 010051)
摘 要: 为了研究纤维和粉煤灰对长 期 浸 泡 作 用 下 聚 乙 烯 醇 纤 维 增 强 水 泥 基 复 合 材 料 (PVA 纤 维/水 泥 复 合 材 料 )抗 硫 酸 钠 侵 蚀 的 影 响 ,对 多 次 试 验 周 期 后 的 试 件 表 观 形 貌 变 化 、质 量 变 化 、体 积 变 化 、抗 压 强 度 和 微 观 结 构 进 行分析研究。试验结果表明,纤维的掺入及良好的分 散,在 水 泥 基 体 中 形 成 了 良 好 的 网 络 分 布 结 构 ,使 PVA 纤 维/水泥复合材料在硫酸钠溶液中的侵蚀速度减缓,但纤维 掺 量 有 一 个 最 佳 值;粉 煤 灰 的 掺 入 在 一 定 程 度 上 密 实 了 PVA 纤维/水泥复合材料,使其抗硫酸钠侵蚀性能得 到 改 善,质 量 分 数 在 50% 之 内 时 随 着 掺 量 的 增 加 而 更 加 明显。 关 键 词 : 聚 乙 烯 醇 纤 维 ;水 泥 基 复 合 材 料 ;抗 硫 酸 盐 侵 蚀 ;质 量 变 化 ;体 积 变 化 ;强 度 变 化 中 图 分 类 号 : TB332 文 献 标 志 码 : A
第 2、4、11、18、25 次 周 期 结 束 后,参 照 GB/T 50081-2002[11]进 行 抗 压 强 度 测 试。 对 25 周 期 结 束后的试件取样,进行扫描电镜(SEM)观 测,对 硫 酸盐损伤 PVA 纤 维/水 泥 复 合 材 料 的 微 观 结 构 进 行分析。
1 实 验 方 法
1.1 原 材 料 与 配 比 试验所采用的基本材料如下:PVA 纤维:日本
Kuraray公司生产的 K- Ⅱ可乐纶,具 体 参 数 如 表 1 所示。水 泥:唐 山 冀 东 水 泥 厂 生 产 的 P.O42.5 级 普通硅酸盐水泥;石英砂:精 选 100~200μm 优 质 石英砂;减水剂:大连 西 卡 建 筑 材 料 有 限 公 司 生 产 的改性 聚 羧 酸 盐 类 高 效 减 水 剂 (Sika Visco Crete 3310E);粉煤灰:内蒙古达拉特旗华宇环保建材 有 限公司生产的Ⅰ 级 粉 煤 灰;增 稠 剂:湖 州 展 望 天 明 药业有限责任公司生产的羟丙基甲基纤维素。
遭受环境因素的侵蚀是导致水泥基材料性能退 化 的 直 接 原 因 之 一 ,硫 酸 盐 侵 蚀 是 水 泥 基 材 料 受 环 境因素作用而发生损伤累积破坏的重要形 式 。 [1] 硫 酸 根 离 子 与 水 泥 水 化 产 物 的 化 学 反 应 、侵 蚀 产 物 的 结 晶 析 出 与 膨 胀 可 对 水 泥 基 材 料 造 成 严 重 破 坏 ,表 现为 膨 胀、开 裂、剥 落 以 及 强 度 损 失 等,这 是 一 个 十分复杂的 物 理 化 学 力 学 变 化 过 程[2]。Al-Dulai- jan等 研 [3] 究 了 混 凝 土 在 不 同 浓 度 硫 酸 钠 溶 液 中 的
0 0 0 0 0 0.1 0.3 0.5
0.4 0.6 0.4 0.6 0.4 0.6 0.4 0பைடு நூலகம்6 0.4 0.6 0.4 0.6 0.4 0.6 0.4 0.6
Fiber volume fraction/% 0 0.5 1 1.5 2 1.5 1.5 1.5
表2 PVA 纤维/水泥复合材料质量比 Table 2 Mass ratio for PVA fiber/cement composites
Number Cement Fly ash Water Quartz sand
F0 F0.5 F1 F1.5 F2 FA1 FA3 FA5
1 1 1 1 1 0.9 0.7 0.5
Resistance of polyvinyl alcohol fiber reinforced cementitious composites to sulfate attack under long-term immersion
LIU Shuguang* ,ZHAO Xiaoming,ZHANG Ju,YANG Changwang
酸 钠 溶 液 中 浸 泡 ,并 使 溶 液 液 面 没 过 试 块 上 表 面 不
小于5cm,以14天 为 一 个 周 期。 每 两 个 周 期 更 换 一次溶液,在2、4、8、11、15、18、22、25 周 期 结 束 后 ,对 试 块 进 行 外 观 拍 照 、质 量 测 量 、体 积 测 量 。
表 1 聚 乙 烯 醇 (PVA)纤 维 的 基 本 特 性
Table 1 Basic characteristics of the polyvinyl alcohol fiber
Density/ Elongation/ Tensile
Elastic
Type
(g·cm-3) %
strength/MPa modulus/GPa
侵蚀 性 能,结 果 表 明,浓 度 越 高,硫 酸 盐 对 混 凝 土 的腐蚀越严重。梁咏宁等 探 [4] 索了硫酸钠和硫 酸 镁 溶 液 对 混 凝 土 的 腐 蚀 破 坏 机 制 ,认 为 两 种 溶 液 对 混 凝 土 侵 蚀 机 制 相 似 ,但 硫 酸 钠 溶 液 对 混 凝 土 的 侵 蚀 更严重。杨 全 兵 等 的 [5] 试 验 结 果 表 明,经 Na2SO4 溶 液 干 湿 循 环 后 ,盐 结 晶 产 生 的 混 凝 土 膨 胀 和 剥 蚀 破坏随着盐浓度和干湿循 环 次数 的 增 加 而增加。 Silderis等 探 [6] 索了 矿 物 掺 和 料 对 混 凝 土 抗 硫 酸 盐
收 到 初 稿 日 期 :2012-12-18;收 到 修 改 稿 日 期 :2013-05-30;网 络 出 版 时 间 :2013-06-21 11:12:00 网 络 出 版 地 址 :www.cnki.net/kcms/detail/11.1801.TB.20130621.1112.008.html 基金项目:国家自然科学基金(50968011;51168033);内蒙古自然 科 学 基 金(2012MS0706;2013MS0709);内 蒙 古 自 治 区 高 等 学 校 科 学 研 究
K- Ⅱ 1.3
6
1600
40
PVA 纤维/水泥复合材料配合比设计如表 2 所 示 ,共 设 计 8 种 配 比 ,144 个 试 件 。 1.2 试 件 制 作 及 试 验 方 法
试验均采用100mm×100 mm×100 mm 立 方 体 试 件 。 试 件 全 部 在 实 验 室 制 备 ,采 用 强 制 式 搅 拌 机搅拌,振动 台 上 完 成 振 捣。 试 件 成 型 24h 后 拆 模 ,在 标 准 养 护 室 (温 度 为 (20±3)℃ ,相 对 湿 度 为 90% 以 上 )中 养 护 28 天 后 进 行 试 验 。
F-Polyvinyl alcohol fiber;A- Fly ash.
参 考 文 献 [10]中 的 试 验 方 法 ,侵 蚀 溶 液 选 用 质 量分数为5%的硫酸 钠 溶 液,采 用 长 期 浸 泡 的 方 法 进 行 硫 酸 盐 侵 蚀 试 验 。 具 体 方 法 是 :将 试 块 置 于 硫
刘 曙 光 ,等 :聚 乙 烯 醇 纤 维 增 强 水 泥 基 复 合 材 料 在 长 期 浸 泡 作 用 下 抗 硫 酸 盐 侵 蚀 性 能
· 61 ·
侵 蚀 性 能 的 影 响 ,发 现 掺 质 量 分 数30% 的 粉 煤 灰 能 提高混凝土抗硫酸盐侵蚀性能。
聚乙 烯 醇 (PVA)纤 维 增 强 水 泥 基 复 合 材 料 (PVA 纤维/水泥复合材料)是一种新型水泥基复合 材料,该 材 料 在 拉 伸、弯 曲、压 缩 等 力 学 性 能 方 面 表现出良好 的 韧 性 和 优 异 的 裂 缝 控 制 能 力[7-9],这 将在一定程度上改善普通混凝土易裂导致的外界有 害物 质 的 侵 入,如 水、氧 气、二 氧 化 碳 以 及 氯 离 子 等较容易进入 混 凝 土 结 构 内 部,引 发 混 凝 土 碳 化、 钢筋锈 蚀,进 而 影 响 钢 筋 混 凝 土 的 寿 命。 目 前, PVA 纤维/水泥复合材料的抗硫酸盐长期浸泡侵蚀 性 能 尚 不 清 楚 ,本 文 中 采 用 不 同 纤 维 掺 量 和 不 同 粉 煤灰掺量的 PVA 纤维/水泥复合材料,研究其经长 期 浸 泡 后 的 质 量 变 化 、体 积 变 化 及 抗 压 强 度 退 化 规 律,并分析了 PVA 纤维/水泥复合材料的抗硫酸盐 长期浸泡侵蚀性能。
复合材料学报 Acta Materiae Compositae Sinica
文 章 编 号 :1000-3851(2013)06-0060-07
第30卷 第6期 12月 2013年 Vol.30 No.6 December 2013
聚乙烯醇纤维增强水泥基复合材料在长期浸泡 作用下抗硫酸盐侵蚀性能
Abstract: In order to research the effect of fiber and fly ash on resistance of polyvinyl alcohol fiber reinforced cementitious composites(PVA fiber/cement composites)to sulfate attack under long-term immersion,the research was done by analyzing morphology change, quality change, volume change, compressive strength and microstructure of the samples tested after several experimental periods.The results of the experiments show that the fiber incorporation with good distribution forming excellent network distribution structure in matrix slows down the erosion rate of PVA fiber/cement composites in sodium sulfate solution,but there is the best content for the fiber incorporation.The fly ash corporation solids PVA fiber/cement composites,and obviously improves resistance of PVA fiber/cement composites to sulfate attack with increasing doping content under mass fraction of 50% . Keywords: polyvinyl alcohol fibers;cementitious composites;sulfate resistance;quality change;volume change; intensity change
项 目 (NJZY12058;13104);内 蒙 古 工 业 大 学 科 学 研 究 项 目 (ZS201137) 通 讯 作 者 :刘 曙 光 ,硕 士 ,教 授 ,博 士 生 导 师 ,主 要 从 事 混 凝 土 基 本 理 论 与 研 究 工 作 E-mail:liusg6011@126.com
刘曙光* ,赵晓明,张 菊,闫长旺
(内蒙古工业大学 矿业学院,呼和浩特 010051)
摘 要: 为了研究纤维和粉煤灰对长 期 浸 泡 作 用 下 聚 乙 烯 醇 纤 维 增 强 水 泥 基 复 合 材 料 (PVA 纤 维/水 泥 复 合 材 料 )抗 硫 酸 钠 侵 蚀 的 影 响 ,对 多 次 试 验 周 期 后 的 试 件 表 观 形 貌 变 化 、质 量 变 化 、体 积 变 化 、抗 压 强 度 和 微 观 结 构 进 行分析研究。试验结果表明,纤维的掺入及良好的分 散,在 水 泥 基 体 中 形 成 了 良 好 的 网 络 分 布 结 构 ,使 PVA 纤 维/水泥复合材料在硫酸钠溶液中的侵蚀速度减缓,但纤维 掺 量 有 一 个 最 佳 值;粉 煤 灰 的 掺 入 在 一 定 程 度 上 密 实 了 PVA 纤维/水泥复合材料,使其抗硫酸钠侵蚀性能得 到 改 善,质 量 分 数 在 50% 之 内 时 随 着 掺 量 的 增 加 而 更 加 明显。 关 键 词 : 聚 乙 烯 醇 纤 维 ;水 泥 基 复 合 材 料 ;抗 硫 酸 盐 侵 蚀 ;质 量 变 化 ;体 积 变 化 ;强 度 变 化 中 图 分 类 号 : TB332 文 献 标 志 码 : A
第 2、4、11、18、25 次 周 期 结 束 后,参 照 GB/T 50081-2002[11]进 行 抗 压 强 度 测 试。 对 25 周 期 结 束后的试件取样,进行扫描电镜(SEM)观 测,对 硫 酸盐损伤 PVA 纤 维/水 泥 复 合 材 料 的 微 观 结 构 进 行分析。
1 实 验 方 法
1.1 原 材 料 与 配 比 试验所采用的基本材料如下:PVA 纤维:日本
Kuraray公司生产的 K- Ⅱ可乐纶,具 体 参 数 如 表 1 所示。水 泥:唐 山 冀 东 水 泥 厂 生 产 的 P.O42.5 级 普通硅酸盐水泥;石英砂:精 选 100~200μm 优 质 石英砂;减水剂:大连 西 卡 建 筑 材 料 有 限 公 司 生 产 的改性 聚 羧 酸 盐 类 高 效 减 水 剂 (Sika Visco Crete 3310E);粉煤灰:内蒙古达拉特旗华宇环保建材 有 限公司生产的Ⅰ 级 粉 煤 灰;增 稠 剂:湖 州 展 望 天 明 药业有限责任公司生产的羟丙基甲基纤维素。
遭受环境因素的侵蚀是导致水泥基材料性能退 化 的 直 接 原 因 之 一 ,硫 酸 盐 侵 蚀 是 水 泥 基 材 料 受 环 境因素作用而发生损伤累积破坏的重要形 式 。 [1] 硫 酸 根 离 子 与 水 泥 水 化 产 物 的 化 学 反 应 、侵 蚀 产 物 的 结 晶 析 出 与 膨 胀 可 对 水 泥 基 材 料 造 成 严 重 破 坏 ,表 现为 膨 胀、开 裂、剥 落 以 及 强 度 损 失 等,这 是 一 个 十分复杂的 物 理 化 学 力 学 变 化 过 程[2]。Al-Dulai- jan等 研 [3] 究 了 混 凝 土 在 不 同 浓 度 硫 酸 钠 溶 液 中 的
0 0 0 0 0 0.1 0.3 0.5
0.4 0.6 0.4 0.6 0.4 0.6 0.4 0பைடு நூலகம்6 0.4 0.6 0.4 0.6 0.4 0.6 0.4 0.6
Fiber volume fraction/% 0 0.5 1 1.5 2 1.5 1.5 1.5
表2 PVA 纤维/水泥复合材料质量比 Table 2 Mass ratio for PVA fiber/cement composites
Number Cement Fly ash Water Quartz sand
F0 F0.5 F1 F1.5 F2 FA1 FA3 FA5
1 1 1 1 1 0.9 0.7 0.5
Resistance of polyvinyl alcohol fiber reinforced cementitious composites to sulfate attack under long-term immersion
LIU Shuguang* ,ZHAO Xiaoming,ZHANG Ju,YANG Changwang
酸 钠 溶 液 中 浸 泡 ,并 使 溶 液 液 面 没 过 试 块 上 表 面 不
小于5cm,以14天 为 一 个 周 期。 每 两 个 周 期 更 换 一次溶液,在2、4、8、11、15、18、22、25 周 期 结 束 后 ,对 试 块 进 行 外 观 拍 照 、质 量 测 量 、体 积 测 量 。
表 1 聚 乙 烯 醇 (PVA)纤 维 的 基 本 特 性
Table 1 Basic characteristics of the polyvinyl alcohol fiber
Density/ Elongation/ Tensile
Elastic
Type
(g·cm-3) %
strength/MPa modulus/GPa
侵蚀 性 能,结 果 表 明,浓 度 越 高,硫 酸 盐 对 混 凝 土 的腐蚀越严重。梁咏宁等 探 [4] 索了硫酸钠和硫 酸 镁 溶 液 对 混 凝 土 的 腐 蚀 破 坏 机 制 ,认 为 两 种 溶 液 对 混 凝 土 侵 蚀 机 制 相 似 ,但 硫 酸 钠 溶 液 对 混 凝 土 的 侵 蚀 更严重。杨 全 兵 等 的 [5] 试 验 结 果 表 明,经 Na2SO4 溶 液 干 湿 循 环 后 ,盐 结 晶 产 生 的 混 凝 土 膨 胀 和 剥 蚀 破坏随着盐浓度和干湿循 环 次数 的 增 加 而增加。 Silderis等 探 [6] 索了 矿 物 掺 和 料 对 混 凝 土 抗 硫 酸 盐
收 到 初 稿 日 期 :2012-12-18;收 到 修 改 稿 日 期 :2013-05-30;网 络 出 版 时 间 :2013-06-21 11:12:00 网 络 出 版 地 址 :www.cnki.net/kcms/detail/11.1801.TB.20130621.1112.008.html 基金项目:国家自然科学基金(50968011;51168033);内蒙古自然 科 学 基 金(2012MS0706;2013MS0709);内 蒙 古 自 治 区 高 等 学 校 科 学 研 究
K- Ⅱ 1.3
6
1600
40
PVA 纤维/水泥复合材料配合比设计如表 2 所 示 ,共 设 计 8 种 配 比 ,144 个 试 件 。 1.2 试 件 制 作 及 试 验 方 法
试验均采用100mm×100 mm×100 mm 立 方 体 试 件 。 试 件 全 部 在 实 验 室 制 备 ,采 用 强 制 式 搅 拌 机搅拌,振动 台 上 完 成 振 捣。 试 件 成 型 24h 后 拆 模 ,在 标 准 养 护 室 (温 度 为 (20±3)℃ ,相 对 湿 度 为 90% 以 上 )中 养 护 28 天 后 进 行 试 验 。
F-Polyvinyl alcohol fiber;A- Fly ash.
参 考 文 献 [10]中 的 试 验 方 法 ,侵 蚀 溶 液 选 用 质 量分数为5%的硫酸 钠 溶 液,采 用 长 期 浸 泡 的 方 法 进 行 硫 酸 盐 侵 蚀 试 验 。 具 体 方 法 是 :将 试 块 置 于 硫
刘 曙 光 ,等 :聚 乙 烯 醇 纤 维 增 强 水 泥 基 复 合 材 料 在 长 期 浸 泡 作 用 下 抗 硫 酸 盐 侵 蚀 性 能
· 61 ·
侵 蚀 性 能 的 影 响 ,发 现 掺 质 量 分 数30% 的 粉 煤 灰 能 提高混凝土抗硫酸盐侵蚀性能。
聚乙 烯 醇 (PVA)纤 维 增 强 水 泥 基 复 合 材 料 (PVA 纤维/水泥复合材料)是一种新型水泥基复合 材料,该 材 料 在 拉 伸、弯 曲、压 缩 等 力 学 性 能 方 面 表现出良好 的 韧 性 和 优 异 的 裂 缝 控 制 能 力[7-9],这 将在一定程度上改善普通混凝土易裂导致的外界有 害物 质 的 侵 入,如 水、氧 气、二 氧 化 碳 以 及 氯 离 子 等较容易进入 混 凝 土 结 构 内 部,引 发 混 凝 土 碳 化、 钢筋锈 蚀,进 而 影 响 钢 筋 混 凝 土 的 寿 命。 目 前, PVA 纤维/水泥复合材料的抗硫酸盐长期浸泡侵蚀 性 能 尚 不 清 楚 ,本 文 中 采 用 不 同 纤 维 掺 量 和 不 同 粉 煤灰掺量的 PVA 纤维/水泥复合材料,研究其经长 期 浸 泡 后 的 质 量 变 化 、体 积 变 化 及 抗 压 强 度 退 化 规 律,并分析了 PVA 纤维/水泥复合材料的抗硫酸盐 长期浸泡侵蚀性能。
复合材料学报 Acta Materiae Compositae Sinica
文 章 编 号 :1000-3851(2013)06-0060-07
第30卷 第6期 12月 2013年 Vol.30 No.6 December 2013
聚乙烯醇纤维增强水泥基复合材料在长期浸泡 作用下抗硫酸盐侵蚀性能