棉纱英文质量标准翻译

合集下载
  1. 1、下载文档前请自行甄别文档内容的完整性,平台不提供额外的编辑、内容补充、找答案等附加服务。
  2. 2、"仅部分预览"的文档,不可在线预览部分如存在完整性等问题,可反馈申请退款(可完整预览的文档不适用该条件!)。
  3. 3、如文档侵犯您的权益,请联系客服反馈,我们会尽快为您处理(人工客服工作时间:9:00-18:30)。

棉纱英文质量标准翻译精梳

40/1s CCW – Combed Compact Weaving

40/1s CCH – Combed Compact Knitting

40/1s CW –Combed Weaving

30/1s CW –Combed Weaving

普梳Carded For Weaving:

20/1s KW – Carded Weaving

24/1s KW

30/1s KW

32/1s KW

36/1s KW

40/1s KW

20/1s OE

Carded For Knitting:

20/1s KH – Carded Knitting

24/1s KH

30/1s KH

32/1s KH –

36/1s KH –

40/1s KH

PARAMETERS 参数20 KW24KW30KW32KW40KW

Actual Count (Ne) 真实支数20s24s30s32s40s

Tolerance 差异(% +/-)1.5 %1.5 %1.5 %1.5 %1.5 %

Count CV% 支数不匀率1.51.51.51.51.5

CSP 缕纱断裂强力24002400240024002400

Strength CV%强力变异系数55555

TPI每寸捻度19.6721.524.0924.8927.82

TPI CV%每寸捻度变异系数55555

U % (UT-3) 乌斯特指数11.211.612.813.213.8

thin幼节/km (-50%)1115273042

thick粗节/km (+50%)7997197220363

Neps棉结/km (+200%)90140316340407

Total Imperfections总疵点/km180252540590812

RKM 断裂长度gm/tex16.016.0161616

Elongation % 伸长% 4.54.54.54.54.25

Rkm CV% 断裂长度变异系数9.09.09.09.09.0

CV% of Elongation 伸长变异系数8.08.08.08.08.0

Hairiness H 毛羽度8.37.87.37.16.3

Classimat Faults偶发性纱疵

Total Faults总纱疵110165220275425

Objectionable Faults A3+B3+C2+D2 (九级纱疵) 55557

H2+I1+I222225

棉纱线长细度指标H2+I1+I2

A.count 支数19.99

C.V.%条干CV 1.16

Lea Str.单纱强力112.24

C.L.S.P.总强力(支数×每磅强力)2243

C.V.%强力CV 3.88

R.K.M千米强力14.35

V.%均匀度10.19

Thin细节1

Thick粗节42

Neps棉节59

CLSP(Count Lea Strength Product)

RKM (Rupture Kilometer)

U % (uniformity %

100% COTTON VIRGIN OE YARNS PRODUCED ON AUTOCORO100%原生棉AUTOCORO(机器型号)气流纺纱

WRAPPING TEST RESULTS经纱测试结果

COUNT纱支

9/1 OE10/1 E12/1 OE16/1 OE

9支单气流纺10支单气流纺12支单气流纺16支单气流纺

Average Count (Ne)平均纱支(英支)

9.019.9611.9415.93

Avg Strength平均强力

214.7197.0159.1115.0

CSP(AROUND)连续纺

1933196318991832

Count Cv%纱支CV%值(Coefficient of variation表示一列数值变异程度的相对指标,是标准差对平均数的百分率)

1.16 1.340.910.99

Strength Cv %强力CV%值

4.12 4.91 3.99

5.48

TPI Test Results TPI测试结果

T.P.I.TWIST PER INCH (每英寸纱线的捻度)

11.3612.4714.0416.65

T.P.I. Cv%TPI CV%值

4.05 4.07 3.95 2.57

T.M.TPM?TWIST PER METER 每米纱线捻度

3.79 3.95

4.06 4.17

Uster Test Results乌斯特测试结果

Avg. U%平均乌斯特值U%

9.6410.1210.019.98

Thin/Km. (-50%))比标准的纱细50%以上的每千米细节数0.20.400.50.0

Thick/Km.(+50%)比标准的纱粗50%以上的每千米粗节数9.423.3032.230.4

Neps/Km.(+280%)比标准的纱粗280%以上的每千米棉结数5.0 6.3019.222.5

Total Imperfections/Km每千米的总瑕疵数

14.630.0051.852.9

Hairiness毛羽

6.03 6.32 6.21 5.02

Sh?

1.58 1.68 1.58 1.31

UTR-3 Test Results UTR-S测试结果

Avg BF (Gms)?

782.5720.2580.1437.2

Avg R.Km (Nm* Kgf).平均千米扭矩?

11.7111.9211.5011.49

.Km Cv %千米CV值

8.487.338.188.65

Elongation %伸长率

6.35 5.98 5.23 5.74

Elongation Cv %伸长率CV值

7.19 6.269.128.02

支数偏差CV100m%(纱线)

绦干均匀度(CV0.01m)%(纱线,粗纱,粗条)

筒管之间差异(CVB%)(纱线)

不均匀指数(纱线)

幼节(-50%)细纱

粗节(+50%)粗节

棉结(+200%~280%)(纱线)

毛羽(H)